# US 2021/0242243 A1 · Metal wiring film and method of fabricating thereof, thin film transistor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0242243 A1
- Document ID: US20210242243A1
- Status: Published application
- Kind: A1
- Application number: 16/631,203
- Filed: 2019-09-17
- Published: 2021-08-05
- Earliest claimed: 2019-04-22
- Assignees: Wuhan China Star Optoelectronics Semiconductor Display Technology Co., Ltd.
- Applicants: Wuhan China Star Optoelectronics Semiconductor Display Technology Co., Ltd.
- Inventors: Toru KIMURA
- Web page: https://patentgrep.com/patent/US20210242243A1

## CPC

- H10D 86/60: wherein the TFTs are in active matrices
- H10D 86/021: {of multiple TFTs}
- H10D 86/441: {Interconnections, e.g. scanning lines}
- H10D: INORGANIC ELECTRIC SEMICONDUCTOR DEVICES

## Abstract

A metal wiring film, a method for fabricating the same, and a thin film transistor. The metal wiring film includes: a first film layer formed by a nickel-copper alloy, a mass percentage of nickel in the nickel-copper alloy ranges from 30% to 70%; a second film layer disposed above the first film layer, a material forming the second film layer is an aluminum-neodymium alloy, and the mass percentage of neodymium in the aluminum-neodymium alloy ranges from 1% to 5%; a third film layer disposed above the second film layer, a material forming the third film layer is the same as the material forming the first film layer.

## Claims

### Claim 1

A metal wiring film, wherein the metal wiring film comprises:
a first film layer formed by a nickel-copper alloy, a mass percentage of nickel in the nickel-copper alloy ranges from 30% to 70%;
a second film layer disposed above the first film layer, a material forming the second film layer is an aluminum-neodymium alloy, and the mass percentage of neodymium in the aluminum-neodymium alloy ranges from 1% to 5%;
a third film layer disposed above the second film layer, a material forming the third film layer is same as the material forming the first film layer.

### Claim 2 (depends on 1)

The metal wiring film according to claim 1, wherein the nickel-copper alloy further comprises metallic titanium, and a mass percentage of titanium in the nickel-copper alloy is between 1% and 10%.

### Claim 3 (depends on 2)

The metal wiring film according to claim 2, wherein the nickel-copper alloy has a mass percentage of nickel of 30%, a mass percentage of copper of 60%, and a mass percentage of titanium of 10%.

### Claim 4 (depends on 1)

The metal wiring film according to claim 1, wherein a mass percentage of neodymium in the aluminum-neodymium alloy is 1%.

### Claim 5 (depends on 1)

The metal wiring film according to claim 1, wherein the first film layer and the third film layer have a same thickness, and a thickness of the second film layer is greater than or equal to twice the sum of a thicknesses of the first film layer and the third film layer.

### Claim 6 (depends on 5)

The metal wiring film according to claim 5, wherein a thickness of the first film layer and the third film layer is between 20 and 60 nm, a thickness of the second film layer is between 200 and 250 nm.

### Claim 7

A thin film translator comprising a metal wiring film, wherein the metal wiring film comprises:
a first film layer formed by a nickel-copper alloy, a mass percentage of nickel in the nickel-copper alloy ranges from 30% to 70%;
a second film layer disposed above the first film layer, a material forming the second film layer is an aluminum-neodymium alloy, and the mass percentage of neodymium in the aluminum-neodymium alloy ranges from 1% to 5%;
a third film layer disposed above the second film layer, a material forming the third film layer is the same as the material forming the first film layer.

### Claim 8 (depends on 7)

The thin film translator according to claim 7, wherein the nickel-copper alloy further comprises metallic titanium, and a mass percentage of titanium in the nickel-copper alloy is between 1% and 10%.

### Claim 9 (depends on 8)

The thin film translator according to claim 8, wherein the nickel-copper alloy has a mass percentage of nickel of 30%, a mass percentage of copper of 60%, and a mass percentage of titanium of 10%.

### Claim 10 (depends on 7)

The thin film translator according to claim 7, wherein a mass percentage of neodymium in the aluminum-neodymium alloy is 1%.

### Claim 11 (depends on 7)

The thin film translator according to claim 7, wherein the first film layer and the third film layer have a same thickness, and a thickness of the second film layer is greater than or equal to twice the sum of a thicknesses of the first film layer and the third film layer.

### Claim 12 (depends on 11)

The thin film translator according to claim 11, wherein a thickness of the first film layer and the third film layer is between 20 and 60 nm, a thickness of the second film layer is between 200 and 250 nm.

### Claim 13

A method of fabricating a metal wiring film in a thin film transistor, wherein the method comprises the following steps:
providing a substrate, the substrate comprising an active region and an insulating layer covering the active region;
forming a transparent conductive film on the insulating layer;
forming a first film layer covering the transparent conductive film, the material of the first film layer is a nickel-copper alloy, and a mass percentage of nickel in the nickel-copper alloy is between 30% and 70%;
forming a second film layer above the first film layer, the material of the second film layer is an aluminum-neodymium alloy, and a mass percentage of neodymium in the aluminum-neodymium alloy is between 1% and 5%;
forming a third film layer over the second film layer, the material of the third film layer is same as the material of the first film layer.

### Claim 14 (depends on 13)

The method of fabricating a metal wiring film according to claim 13, wherein the method of forming the first film layer and the third film layer is:
providing a vacuum chamber, the pressure of the vacuum chamber is less than or equal to 4×10−5 Pa;
pouring argon into the vacuum chamber such that the pressure in the vacuum chamber is between 0.2 and 1 Pa;
using a nickel-copper alloy film as a target of a direct current sputtering method to form a nickel-copper alloy film having a thickness ranging from 20 to 60 nm.

### Claim 15 (depends on 13)

The method of fabricating a metal wiring film according to claim 13, wherein the method of forming the second film layer is:
providing a vacuum chamber, the pressure of the vacuum chamber is less than or equal to 4×10−5 Pa;
pouring argon into the vacuum chamber such that the pressure in the vacuum chamber is between 0.2 and 1 Pa;
forming an aluminum-niobium alloy film having a thickness ranging from 200 to 250 nm by a direct current sputtering method using an aluminum-niobium alloy as a target.