# US 2021/0178459 A1 · Use of a coating composition and corresponding method for producing a centrifugal casting mould with a coating

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0178459 A1
- Document ID: US20210178459A1
- Status: Published application
- Kind: A1
- Application number: 17/268,015
- Filed: 2019-08-13
- Published: 2021-06-17
- Earliest claimed: 2018-08-13
- Assignees: HÜTTENES-A-ALBERTUS Chemische Werke Gesellschaft mit beschränkte Haftung
- Applicants: HÜTTENES-A-ALBERTUS Chemische Werke Gesellschaft mit beschränkte Haftung
- Inventors: Sven Hennig; Andreas Jattke; Klaus Seeger
- Web page: https://patentgrep.com/patent/US20210178459A1

## CPC

- B22C 3/00: Selection of compositions for coating the surfaces of moulds, cores, or patterns
- B05D 1/02: performed by spraying
- B22C 9/06: Permanent moulds for shaped castings (moulds for ingots B22D7/06)
- B22D 13/102: {Linings for moulds (making or lining moulds B22C)}
- C04B 35/481: {containing silicon, e.g. zircon}
- C04B 35/482: Refractories from grain sized mixtures
- C04B 35/62222: {obtaining ceramic coatings (coating of mortars, concrete, artificial or natural stone or ceramics C04B41/45; laminated ceramic products B32B18/00; coating of glass C03C17/00, applying ceramic coatings on silicon for semi-conductor purposes H10W; coating metallic materials C23)}
- C04B 2235/3248: Zirconates or hafnates, e.g. zircon
- C04B 2235/3418: Silicon oxide, silicic acids or oxide forming salts thereof, e.g. silica sol, fused silica, silica fume, cristobalite, quartz or flint
- C04B 2235/422: Carbon
- C04B 2235/528: Spheres
- C04B 2235/5436: micrometer sized, i.e. from 1 to 100 micron
- B22C: FOUNDRY MOULDING (moulding refractory materials in general B28B)
- B05D: PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL (conveying articles or workpieces through baths of liquid B65G, e.g. B65G49/02)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE

## Abstract

A description is given of the use of a refractory coating composition having a solids fraction of more than 69 wt %, based on the total mass of the coating composition, and also having a loss on ignition of less than 0.6 wt %, based on the total mass of the solids fraction of the coating composition, for producing a refractory coating on the inner walls of a centrifugal casting mold by means of a spray application. Further described is a method for producing a centrifugal casting mold provided on its inner walls with a refractory coating, for use in the centrifugal casting process, and also a method for producing a casting in the centrifugal casting process, preferably having a structured surface. Also described is a centrifugal casting mold for use in the centrifugal casting process, having a refractory coating on the inner walls of the centrifugal casting mold.

## Claims

### Claim 1

A method of producing a refractory coating on the inner walls of a centrifugal casting mold by means of a spray application of a refractory coating composition, wherein the refractory coating composition has:
a solids fraction of more than 69 wt %, based on the total mass of the coating composition, and
a loss on ignition of less than 0.6 wt %, based on the total mass of the solids fraction of the coating composition,
wherein the refractory coating composition is a dispersion of refractories in an aqueous phase, the refractories at least comprising
(a)—a total amount in the range from 4 to 50 wt % of particulate amorphous oxide, based on the total mass of the coating composition,
wherein the particulate amorphous oxide comprises a fraction of 85 wt % or more of silicon dioxide, based on the total amount of the particulate amorphous oxide,
wherein the particulate amorphous oxide possesses a mass-based D95 of less than 5 μm, determined by laser diffraction,
wherein the particulate amorphous oxide possesses a porosity of less than 50%, based on the total amount of the particulate amorphous oxide, and
wherein 90 wt % or more of the particles of the particulate amorphous oxide possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images, or
a total amount in the range from 4 to 50 wt % of microsilica as particulate amorphous oxide, based on the total mass of the coating composition, and
(b) one or more further refractories,
wherein 98 wt % or more of the total mass of the refractories are capable of passing through a sieve having a mesh size of 0.75 mm.

### Claim 2 (depends on 1)

The method as claimed in claim 1, wherein the particulate amorphous oxide of constituent (a) possesses a loss on ignition of less than 0.6 wt %, based on the total amount of the particulate amorphous oxide of constituent (a).

### Claim 3 (depends on 1)

The method as claimed in claim 1, wherein
the coating composition comprises (i) zirconium oxide, (ii) carbon and/or (iii) a Lewis acid, preferably as secondary constituents from the preparation of the particulate amorphous oxide of constituent (a),
and/or
the particulate amorphous oxide of constituent (a) comprises a fraction of 90 wt % of silicon dioxide or more, based in each case on the total amount of the particulate amorphous oxide of constituent (a).

### Claim 4 (depends on 1)

The method as claimed in claim 1, wherein
90 wt % or more of the particles of the particulate amorphous oxide of constituent (a) possess a sphericity of greater than 0.95, determined by evaluating two-dimensional microscope images,
and/or
wherein the particulate amorphous oxide of constituent (a) possesses a mass-based D95 of less than 3 μm, determined by laser diffraction.

### Claim 5 (depends on 1)

The method as claimed in claim 1, wherein the particulate amorphous oxide of constituent (a) comprises one or more constituents selected from the group consisting of
silicon dioxide particles which are preparable by spraying a silicon dioxide melt, and
microsilica.

### Claim 6 (depends on 1)

The method as claimed in claim 1, wherein the particulate amorphous oxide of constituent (a) comprises a fraction of 85 wt % or more of microsilica, based in each case on the total amount of the particulate amorphous oxide of constituent (a).

### Claim 7 (depends on 1)

The method as claimed in claim 1, wherein
the particles of the particulate amorphous oxide of constituent (a) possess a pozzolanic activity.

### Claim 8 (depends on 1)

The method as claimed in claim 1,
wherein the refractory coating composition comprises a total amount in the range from 4 to 25 wt % of particulate amorphous oxide of constituent (a), based on the total mass of the coating composition, and/or
wherein the total fraction of particulate amorphous oxides of constituent (a) is less than 50 wt %, based on the total amount of the refractories in the coating composition.

### Claim 9 (depends on 1)

The method as claimed in claim 1, wherein the refractory coating composition
comprises one or more surface-active substances.

### Claim 10 (depends on 1)

The method as claimed in claim 1,
wherein the fraction of crystalline silicon dioxide is less than 3 wt %, based on the total mass of the coating composition, and/or
wherein the total fraction of zirconium silicates and zirconium oxide is less than 7 wt %, based on the total mass of the coating composition, and/or
wherein the fraction of α-alumina is less than 5 wt %, based on the total mass of the coating composition, and/or
wherein the fraction of refractories having a Mohs hardness of more than 7 is less than 5 wt %, based on the total mass of the coating composition, and/or
wherein the fraction of diatomaceous earth is less than 10 wt %, based on the total amount of the particulate amorphous oxide of constituent (a).

### Claim 11 (depends on 1)

The method as claimed in claim 1, wherein the refractory coating composition comprises an inorganic binder.

### Claim 12 (depends on 1)

The method as claimed in claim 1, wherein the refractory coating composition
comprises one or more rheological additives, and/or
comprises one or more biocides.

### Claim 13 (depends on 1)

The method as claimed in claim 1, wherein the refractory coating composition comprises one or more rheological additives,
wherein a fraction of rheological additives is selected such that this fraction possesses a loss on ignition of less than 0.5 wt %, based on the total mass of the solids fraction of the coating composition.

### Claim 14 (depends on 1)

The method as claimed in claim 1, wherein the refractory coating composition comprises in the aqueous phase an alcohol having a boiling point of less than 100° C. at 1013 hPa, and preferably comprises ethanol in the aqueous phase.

### Claim 15 (depends on 1)

The method as claimed in claim 1, wherein the one or more further refractories of constituent (b) comprise one or more constituents selected from the group consisting of
hollow particles which possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images,
wherein the fraction of these hollow particles is in the range from 0.1 to 10 wt %, based on the total mass of the coating composition,
ceramic particles which possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images.

### Claim 16 (depends on 1)

The method as claimed in claim 1, wherein a refractory coating composition is used
having a solids fraction of more than 69 wt %, based on the total mass of the coating composition, and
having a loss on ignition of less than 0.6 wt %, based on the total mass of the solids fraction of the coating composition,
wherein the coating composition is a dispersion of refractories in an aqueous phase, the refractories at least comprising
(a)—a total amount in the range from 4 to 50 wt % of particulate amorphous oxide, based on the total mass of the coating composition,
wherein the particulate amorphous oxide comprises a fraction of 85 wt % or more of silicon dioxide, based on the total amount of the particulate amorphous oxide,
wherein the particulate amorphous oxide possesses a mass-based D95 of less than 5 μm, determined by laser diffraction,
wherein the particulate amorphous oxide possesses a porosity of less than 50%, based on the total amount of the particulate amorphous oxide, and
wherein 90 wt % or more of the particles of the particulate amorphous oxide possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images,
or
a total amount in the range from 4 to 50 wt % of microsilica as particulate amorphous oxide, based on the total mass of the coating composition,
and
(b) one or more further refractories,
wherein the coating composition comprises:
one or more surface-active substances,
an inorganic binder, and
one or more rheological additives.

### Claim 17 (depends on 1)

The method as claimed in claim 1, wherein the solids fraction of the refractory coating composition is in the range from more than 69 wt % to a maximum of 80 wt %, based on the total mass of the coating composition.

### Claim 18 (depends on 1)

The method as claimed in claim 1, wherein the solids fraction of the refractory coating composition is in the range from more than 69 wt % to a maximum of 75 wt %, based on the total mass of the coating composition.

### Claim 19 (depends on 1)

The method as claimed in claim 1, wherein the refractory coating on the inner walls of the centrifugal casting mold possesses a negative structure, for producing a metallic casting having a structured surface.

### Claim 20 (depends on 1)

The method as claimed in claim 1, wherein the spray application at least in regions of the inner walls is made in two or more coats, the application of the second or at least one of the further coats taking place onto a previously applied, preferably not fully dried coat of the refractory coating.

### Claim 21

A method for producing a centrifugal casting mold provided on its inner walls with a refractory coating, for use in the centrifugal casting process, having the following steps:
providing or producing a refractory coating composition,
applying one or more coats of the provided or produced coating composition to the inner walls of the centrifugal casting mold, preferably with the centrifugal casting mold rotating and/or heated, where preferably the resulting refractory coating at least after drying possesses a negative structure for producing a casting having a structured surface,
wherein the refractory coating composition is a dispersion of refractories in an aqueous phase, the refractories at least comprising
(a)—a total amount in the range from 4 to 50 wt % of particulate amorphous oxide, based on the total mass of the coating composition,
wherein the particulate amorphous oxide comprises a fraction of 85 wt % or more of silicon dioxide, based on the total amount of the particulate amorphous oxide,
wherein the particulate amorphous oxide possesses a mass-based D95 of less than 5 μm, determined by laser diffraction,
wherein the particulate amorphous oxide possesses a porosity of less than 50%, based on the total amount of the particulate amorphous oxide, and
wherein 90 wt % or more of the particles of the particulate amorphous oxide possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images, or
a total amount in the range from 4 to 50 wt % of microsilica as particulate amorphous oxide, based on the total mass of the coating composition, and
(b) one or more further refractories,
wherein 98 wt % or more of the total mass of the refractories are capable of passing through a sieve having a mesh size of 0.75 mm.

### Claim 22

A method for producing a casting in the centrifugal casting process, comprising the steps of:
providing or producing a refractory coating composition,
applying one or more coats of the provided or produced coating composition to the inner walls of a centrifugal casting mold, to produce a refractory coating,
introducing the casting metal into the rotating centrifugal casting mold whose inner walls have been coated,
solidifying the casting in the rotating centrifugal casting mold,
extracting the casting from the centrifugal casting mold,
wherein the refractory coating composition is a dispersion of refractories in an aqueous phase, the refractories at least comprising
(a)—a total amount in the range from 4 to 50 wt % of particulate amorphous oxide, based on the total mass of the coating composition,
wherein the particulate amorphous oxide comprises a fraction of 85 wt % or more of silicon dioxide, based on the total amount of the particulate amorphous oxide,
wherein the particulate amorphous oxide possesses a mass-based D95 of less than 5 μm, determined by laser diffraction,
wherein the particulate amorphous oxide possesses a porosity of less than 50%, based on the total amount of the particulate amorphous oxide, and
wherein 90 wt % or more of the particles of the particulate amorphous oxide possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images, or
a total amount in the range from 4 to 50 wt % of microsilica as particulate amorphous oxide, based on the total mass of the coating composition, and
(b) one or more further refractories,
wherein 98 wt % or more of the total mass of the refractories are capable of passing through a sieve having a mesh size of 0.75 mm.

### Claim 23

A centrifugal casting mold for use in the centrifugal casting process, having a refractory coating on the inner walls of the centrifugal casting mold,
wherein the refractory coating has dried,
wherein the refractory coating consists of those constituents of a refractory coating composition that are not vaporizable at 1013 hPa and a temperature of 105° C.,
wherein the refractory coating is a dried dispersion of the refractory coating composition in an aqueous phase, wherein the refractory coating composition comprises:
(a)—a total amount in the range from 4 to 50 wt % of particulate amorphous oxide, based on the total mass of the coating composition,
wherein the particulate amorphous oxide comprises a fraction of 85 wt % or more of silicon dioxide, based on the total amount of the particulate amorphous oxide,
wherein the particulate amorphous oxide possesses a mass-based D95 of less than 5 μm, determined by laser diffraction,
wherein the particulate amorphous oxide possesses a porosity of less than 50%, based on the total amount of the particulate amorphous oxide, and
wherein 90 wt % or more of the particles of the particulate amorphous oxide possess a sphericity of greater than 0.9, determined by evaluating two-dimensional microscope images, or
a total amount in the range from 4 to 50 wt % of microsilica as particulate amorphous oxide, based on the total mass of the coating composition, and
(b) one or more further refractories,
wherein 98 wt % or more of the total mass of the refractories are capable of passing through a sieve having a mesh size of 0.75 mm.