# US 2021/0172071 A1 · Hard and wear resistant titanium alloy and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0172071 A1
- Document ID: US20210172071A1
- Status: Published application
- Kind: A1
- Application number: 16/703,960
- Filed: 2019-12-05
- Published: 2021-06-10
- Earliest claimed: 2019-12-05
- Inventors: Monireh Ganjali; Pouya Karimyan
- Web page: https://patentgrep.com/patent/US20210172071A1

## CPC

- C23D 5/02: by wet methods
- B32B 15/04: comprising metal as the main or only constituent of a layer, {which is} next to another layer of {the same or of} a {different material (next to a bituminous or tarry layer B32B11/08; next to a water-setting substance layer B32B13/06; next to a glass layer B32B17/061; next to a cellulosic plastic layer B32B23/042)}
- C03C 3/095: containing rare earths
- C03C 8/02: Frit compositions, i.e. in a powdered or comminuted form
- C03C 8/14: Glass frit mixtures having non-frit additions, e.g. opacifiers, colorants, mill-additions
- C03C 10/0018: {containing SiO2, Al2O3 and monovalent metal oxide as main constituents}
- C03C 10/0054: {containing PbO, SnO2, B2O3}
- C22C 14/00: Alloys based on titanium
- C03C 2204/00: Glasses, glazes or enamels with special properties
- C23D: ENAMELLING OF, OR APPLYING A VITREOUS LAYER TO, METALS
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

The present invention discloses a hard and wear resistant titanium alloy and a method of preparing the hard and wear resistant titanium alloy utilizing laser cladding method. A glass-ceramic composite of SiO2—Al2O3—ZrO2—Y2O3—K2O—Na2O—B2O3 is coated on titanium alloy Ti-6Al-4V substrate utilizing laser cladding. The laser cladding method replaces the need of industrial furnaces and reduces the amount of pollutants entering the atmosphere. The titanium Ti-6Al-4V alloy coated with the glass ceramic composite could be used in the aviation and maritime industries, instead of nickel and cobalt-based superalloys, to significantly reduce costs.

## Claims

### Claim 1

A method of preparing hard and wear resistant titanium alloy, comprising the steps of:
preparing a Ti-6Al-4V substrate;
preparing a glass-ceramic slurry of SiO2—Al2O3—ZrO2—Y2O3—K2O—Na2O—B2O3;
spraying the slurry onto the Ti-6Al-4V substrate;
drying the slurry on the Ti-6Al-4V substrate, and
applying a continuous wave of CO2 laser to form the titanium alloy.

### Claim 2 (depends on 1)

The method of claim 1, wherein the step of preparing Ti-6Al-4V substrate includes:
a) providing one or more Ti-6Al-4V plates with dimensions of 30×10×1 mm;
b) grounding the plates with silicon carbide papers of 400-2000 grit;
c) polishing a mixture obtained at step (b) with 5m diamond paste;
d) treating a mixture obtained at step (c) using a sandblast method, and
e) cleaning and drying a mixture obtained at step (d) to form the Ti-6Al-4V substrate.

### Claim 3 (depends on 1)

The method of claim 1, wherein the step of preparing the glass-ceramic slurry of SiO2—Al2O3—ZrO2—Y2O3—K2O—Na2O—B2O3 includes:
a) mixing raw glass materials including silicon dioxide (SiO2), yttrium (III) oxide (Y2O3), potassium carbonate (K2CO3), sodium carbonate (Na2CO3), zirconium dioxide (ZrO2), boric acid (H3BO3), and aluminum oxide (Al2O3);
b) mixing at least one of ethanol or water with the mixture obtained at step (a) in 2:1 ratio, and
c) adding 1.5 g of 1% CMC adhesive to a mixture obtained at step (b) and grounded to form the glass-ceramic slurry.

### Claim 4 (depends on 1)

The method of claim 1, wherein the CO2 laser comprises an operating wavelength of 10.6 nm, a laser beam diameter of 2 mm, and an output power of 70-100 W with scanning speed 1-3 mm/s.

### Claim 5 (depends on 1)

The method of claim 1, wherein the glass-ceramic slurry comprises silicon dioxide (SiO2) of 51 mole %, yttrium (III) oxide (Y2O3) of 2.4 mole %, potassium carbonate (K2CO3) of 4 mole %, sodium carbonate (Na2CO3) of 6 mole %, zirconium dioxide (ZrO2) of 5.6 mole %, boric acid (H3BO3) of 20 mole %, and aluminum oxide (Al2O3) of 11 mole %.

### Claim 6 (depends on 1)

The method of claim 1, wherein the Ti-6Al-4V substrate comprises aluminum (Al) of 5.83 wt %, vanadium (V) is 3.86 wt %, copper (Cu) of 0.15 wt %, molybdenum (Mo) of 0.43 wt %, stannum (Sn) of 0.35 wt %, niobium (Nb) of 0.35 wt %, palladium (Pd) of 0.15 wt %, iron (Fe) of 0.15 wt %, and titanium (Ti) of 90 wt %.

### Claim 7

A hard and wear resistant titanium alloy, comprising:
a Ti-6Al-4V substrate coated by a glass-ceramic composite of SiO2—Al2O3—ZrO2—Y2O3—K2O—Na2O—B2O3,
wherein the composite comprises silicon dioxide (SiO2) of 51 mole %, yttrium (III) oxide (Y2O3) of 2.4 mole %, potassium carbonate (K2CO3) of 4 mole %, sodium carbonate (Na2CO3) of 6 mole %, zirconium dioxide (ZrO2) of 5.6 mole %, boric acid (H3BO3) of 20 mole %, and aluminum oxide (Al2O3) of 11 mole %, and
wherein the substrate comprises aluminum (Al) of 5.83 wt %, vanadium (V) is 3.86 wt %, copper (Cu) of 0.15 wt %, molybdenum (Mo) of 0.43 wt %, stannum (Sn) of 0.35 wt %, niobium (Nb) of 0.35 wt %, palladium (Pd) of 0.15 wt %, iron (Fe) of 0.15 wt %, and titanium (Ti) of 90 wt %.

### Claim 8 (depends on 1)

The titanium alloy of claim 1, wherein the glass-ceramic composite is coated to the Ti-6Al-4V substrate by laser cladding method.

### Claim 9 (depends on 1)

The titanium alloy of claim 1, wherein the glass-ceramic composite is coated to the Ti-6Al-4V substrate by applying a continuous wave of CO2 laser.

### Claim 10 (depends on 9)