# US 2021/0171813 A1 · Radical-polymerizable adhesive composition for laminating and bonding steel plates, adhesive laminate, motor, and method for manufacturing adhesive laminate

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0171813 A1
- Document ID: US20210171813A1
- Status: Published application
- Kind: A1
- Application number: 16/769,864
- Filed: 2018-11-09
- Published: 2021-06-10
- Earliest claimed: 2017-12-18
- Assignees: Threebond Co., Ltd.
- Applicants: Threebond Co., Ltd.
- Inventors: Satoshi KANEKO
- Web page: https://patentgrep.com/patent/US20210171813A1

## CPC

- C09J 151/08: grafted on to macromolecular compounds obtained otherwise than by reactions only involving carbon-to-carbon unsaturated bonds
- C09J 175/14: Polyurethanes having carbon-to-carbon unsaturated bonds
- B32B 7/12: using interposed adhesives or interposed materials with bonding properties
- B32B 15/043: {of metal (B32B15/01 takes precedence)}
- B32B 15/08: of synthetic resin
- B32B 15/082: comprising vinyl resins; comprising acrylic resins
- B32B 15/18: comprising iron or steel {(B32B15/011, B32B15/012 and B32B15/013 take precedence)}
- B32B 37/12: characterised by using adhesives
- C08F 220/20: of polyhydric alcohols or phenols {, e.g. 2-hydroxyethyl (meth)acrylate or glycerol mono-(meth)acrylate}
- C08F 290/064: {Polymers containing more than one epoxy group per molecule}
- C08F 290/067: {Polyurethanes; Polyureas}
- C09J 4/00: Adhesives based on organic non-macromolecular compounds having at least one polymerisable carbon-to-carbon unsaturated bond {; adhesives, based on monomers of macromolecular compounds of groups C09J183/00 - C09J183/16}
- C09J 4/06: {Organic non-macromolecular compounds having at least one polymerisable carbon-to-carbon unsaturated bond} in combination with a macromolecular compound other than an unsaturated polymer of groups C09J159/00 - C09J187/00
- C09J 11/06: organic
- C09J 163/10: Epoxy resins modified by unsaturated compounds
- H02K 15/02: of stator or rotor bodies
- B32B 2311/30: Iron, e.g. steel
- C09J 2400/20: Presence of organic materials
- C09J 2463/00: Presence of epoxy resin
- C09J 2475/00: Presence of polyurethane
- C09J: ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES (preparation of glue or gelatine C09H)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- H02K: DYNAMO-ELECTRIC MACHINES (dynamo-electric relays H01H53/00; conversion of DC or AC input power into surge output power {H03K3/53})

## Abstract

An object of the present invention is to provide a radical-polymerizable adhesive composition for laminating and bonding steel plates, capable of obtaining an adhesive laminate that contributes to simplification of a process in an adhesive lamination method, and high performance and high reliability of a rotor or a stator of a motor. A radical-polymerizable adhesive composition for laminating and bonding steel plates, exhibiting a value of 8.0 MPa or more in a tensile shear adhesive strength test to an electromagnetic steel plate, and containing: component (A): a radical-polymerizable compound; component (B): a radical-polymerization initiator; and component (C): a phosphate compound having a group represented by the following general formula (1) or (2).

## Claims

### Claim 1

A radical-polymerizable adhesive composition for laminating and bonding steel plates, exhibiting a value of 8.0 MPa or more in a following tensile shear adhesive strength test to an electromagnetic steel plate, and comprising:
component (A): a radical-polymerizable compound; component (B): a radical-polymerization initiator; and component (C): a phosphate compound having a group represented by the following general formula (1) or (2):
the tensile shear adhesive strength test to the electromagnetic steel plate is as follows:
to a test piece of an electromagnetic steel plate having a width of 25 mm, a length of 100 mm, and a thickness of 0.3 mm, 0.1 g of a primer composition containing 100 parts by mass of punching oil, 100 parts by mass of ethanol, and 0.5 part by mass of copper 2-ethylhexanoate is applied, and is left and dried at 25° C. for three hours,
next, to the test piece that has been subjected to the primer treatment, 0.1 g of the radical-polymerizable adhesive composition for laminating and bonding steel plates is applied, another test piece that has been subjected to the primer treatment is superimposed thereon such that a length of a longer side end thereof is 10 mm, and a weight of 100 g is placed on a bonding surface and fixed at 25° C. for 24 hours to obtain an adhesion test piece,
next, an end of the adhesion test piece is pulled with a universal tensile tester at a pulling speed of 50 mm/min, and tensile shear adhesive strength (MPa) is measured according to JIS K6850 (1999).

### Claim 2 (depends on 1)

The radical-polymerizable adhesive composition for laminating and bonding steel plates according to claim 1, wherein the component (A) contains at least a radical-polymerizable oligomer or a radical-polymerizable polymer.

### Claim 3 (depends on 1)

The radical-polymerizable adhesive composition for laminating and bonding steel plates according to claim 1, wherein the component (A) contains at least one selected from the group consisting of a urethane (meth)acrylate, an epoxy (meth)acrylate, an ester (meth)acrylate, an isoprene-based (meth)acrylate, a hydrogenated isoprene-based (meth)acrylate, a (meth)acrylic group-containing acrylic polymer, and a (meth)acrylic group-containing polyisobutylene.

### Claim 4 (depends on 1)

The radical-polymerizable adhesive composition for laminating and bonding steel plates according to claim 1, wherein the component (A) contains a urethane (meth)acrylate or an epoxy (meth)acrylate.

### Claim 5 (depends on 1)

The radical-polymerizable adhesive composition for laminating and bonding steel plates according to claim 1, further comprising an anaerobic catalyst as a component (D).

### Claim 6 (depends on 1)

The radical-polymerizable adhesive composition for laminating and bonding steel plates according to claim 1, wherein a glass transition point of a cured product of the radical-polymerizable adhesive composition is 60° C. or higher.

### Claim 7 (depends on 1)

The radical-polymerizable adhesive composition for laminating and bonding steel plates according to claim 1, having a viscosity of 30 Pa·s or less.

### Claim 8 (depends on 1)

An adhesive laminate obtained by laminating electromagnetic steel plates using the radical-polymerizable adhesive composition for laminating and bonding steel plates set forth in claim 1.

### Claim 9 (depends on 8)

A motor using the adhesive laminate set forth in claim 8.

### Claim 10

A method for manufacturing an adhesive laminate, comprising: applying a radical-polymerizable adhesive composition for laminating and bonding steel plates exhibiting a value of 8.0 MPa or more in a following tensile shear adhesive strength test to an electromagnetic steel plate to a surface of a strip-shaped steel plate; and laminating electromagnetic steel plates with a press molding machine,
the tensile shear adhesive strength test to the electromagnetic steel plate is as follows:
to a test piece of an electromagnetic steel plate having a width of 25 mm, a length of 100 mm, and a thickness of 0.3 mm, 0.1 g of a primer composition containing 100 parts by mass of punching oil, 100 parts by mass of ethanol, and 0.5 part by mass of copper 2-ethylhexanoate is applied, and is left and dried at 25° C. for three hours,
next, to the test piece that has been subjected to the primer treatment, 0.1 g of the radical-polymerizable adhesive composition for laminating and bonding steel plates is applied, another test piece that has been subjected to the primer treatment is superimposed thereon such that a length of a longer side end thereof is 10 mm, and a weight of 100 g is placed on a bonding surface and fixed at 25° C. for 24 hours to obtain an adhesion test piece,
next, an end of the adhesion test piece is pulled with a universal tensile tester at a pulling speed of 50 mm/min, and tensile shear adhesive strength (MPa) is measured according to JIS K6850 (1999).

### Claim 11 (depends on 10)

The method for manufacturing an adhesive laminate according to claim 10, wherein the radical-polymerizable adhesive composition for laminating and bonding steel plates contains: component (A): a radical-polymerizable compound; component (B): a radical-polymerization initiator; and component (C): a phosphate compound having a group represented by the following general formula (1) or (2):