# US 2021/0079559 A1 · Modified cross-section fiber and method for manufacturing same and nonwoven fabric and noise-absorbing and -insulating material comprising modified cross-section fiber

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0079559 A1
- Document ID: US20210079559A1
- Status: Published application
- Kind: A1
- Application number: 17/104,280
- Filed: 2020-11-25
- Published: 2021-03-18
- Earliest claimed: 2018-05-29
- Assignees: Mitsubishi Chemical Corporation
- Applicants: Mitsubishi Chemical Corporation
- Inventors: Tatsuhiko INAGAKI
- Web page: https://patentgrep.com/patent/US20210079559A1

## CPC

- D01D 5/253: with a non-circular cross section; Spinnerette packs therefor (D01D5/38 takes precedence)
- D04H 1/43838: {Ultrafine fibres, e.g. microfibres}
- D04H 1/43912: {fibres with noncircular cross-sections}
- D04H 3/016: characterised by the fineness
- D04H 3/018: characterised by the shape
- E04B 1/8409: {sheet-shaped}
- G10K 11/162: Selection of materials
- D06M 2101/32: Polyesters
- D01D: MECHANICAL METHODS OR APPARATUS IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS
- D04H: MAKING TEXTILE FABRICS, e.g. FROM FIBRES OR FILAMENTARY MATERIAL (weaving D03; knitting D04B; braiding D04C; net-making D04G; sewing D05B; tufting D05C; finishing non-woven fabrics D06); FABRICS MADE BY SUCH PROCESSES OR APPARATUS, e.g. FELTS, NON-WOVEN FABRICS; COTTON-WOOL; WADDING {; NON-WOVEN FABRICS FROM STAPLE FIBRES, FILAMENTS OR YARNS, BONDED WITH AT LEAST ONE WEB-LIKE MATERIAL DURING THEIR CONSOLIDATION}(non-woven fabrics having an intermediate or external layer of a different kind, e.g. of woven fabric, B32B)
- E04B: GENERAL BUILDING CONSTRUCTIONS; WALLS, e.g. PARTITIONS; ROOFS; FLOORS; CEILINGS; INSULATION OR OTHER PROTECTION OF BUILDINGS (border constructions of opening in walls, floors or ceilings E06B1/00; {electromagnetic shielding H05K9/0001})
- G10K: SOUND-PRODUCING DEVICES; METHODS OR DEVICES FOR PROTECTING AGAINST, OR FOR DAMPING, NOISE OR OTHER ACOUSTIC WAVES IN GENERAL; ACOUSTICS NOT OTHERWISE PROVIDED FOR
- D06M: TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS

## Abstract

The invention provides a modified cross-section fiber is provided having a single fiber fineness of 0.01 to 1.0 dtex and modified cross-section degree (α, α=P/(4πA)1/2, where P represents a peripheral length (μm) in a fiber cross section, and A represents an area of the fiber cross section (μm2)) of 1.5 to 4.0 at a fiber cross section taken along a direction perpendicular to the fiber axis.

## Claims

### Claim 1

A modified cross-section fiber having a single fiber fineness of 0.01 to 1.0 dtex and modified cross-section degree (α) of 1.5 to 4.0 at a fiber cross section taken along a direction perpendicular to a fiber axis,
wherein the non-circularity degree is calculated by Equation (1),
α=P/(4πA)1/2 (1)
in the equation, P is a peripheral length (unit: μm) of the fiber cross section, and A is an area of the fiber cross section (unit: μm2).

### Claim 2 (depends on 1)

The modified cross-section fiber according to claim 1, wherein the area (A) of the fiber cross section is 0.5 to 100 μm2, and the peripheral length (P) in the fiber cross section is 5 to 250 μm.

### Claim 3 (depends on 1)

The modified cross-section fiber according to claim 1, wherein the fiber cross section is Y-shaped, cross-shaped, 6-lobed, 8-lobed, or pinwheel-shaped.

### Claim 4 (depends on 1)

The modified cross-section fiber according to claim 1, which is a polyester fiber, a polypropylene fiber, a nylon fiber, an aramid fiber, an acrylic fiber, or a rayon fiber.

### Claim 5 (depends on 1)

The modified cross-section fiber according to claim 1 having a noise absorption coefficient equal to or higher than 0.40 at a frequency of 400 to 1,250 Hz, wherein the noise absorption coefficient is measured in a noise-absorbing and -insulating performance test (I), the noise-absorbing and -insulating performance test (I) comprising:
cutting a fiber (0.81 g) in a length of 40 mm;
putting the cut fiber in a cylindrical holder having a diameter of 41.5 mm and a thickness of 30 mm;
measuring a normal incidence noise absorption coefficient at a frequency of 400 to 1,250 Hz; and
calculating an average of the coefficient.

### Claim 6 (depends on 1)

The modified cross-section fiber according to claim 1 having a noise absorption coefficient equal to or higher than 0.17 at a frequency of 400 to 1,250 Hz, wherein the noise absorption coefficient is measured in a noise-absorbing and -insulating performance test (II), the noise-absorbing and -insulating performance test (II) comprising:
cutting a fiber (0.27 g) in a length of 40 mm;
putting the cut fiber in a cylindrical holder having a diameter of 41.5 mm and a thickness of 20 mm;
measuring a normal incidence noise absorption coefficient at a frequency of 400 to 1,250 Hz; and
calculating an average of the coefficient.

### Claim 7 (depends on 1)

The modified cross-section fiber according to claim 1 having a transmission loss equal to or higher than 5.1 dB at a frequency of 400 to 5,000 Hz, wherein the transmission loss is measured in a noise-absorbing and -insulating performance test (III), the noise-absorbing and -insulating performance test (III) comprising:
mixing the modified cross-section fiber (70% by mass) having a fiber length of 40 mm with 30% by mass of a polyester melting fiber having a single fiber fineness of 2.2 dtex, a fiber length of 51 mm, and a melting point of 110° C.;
heating the mixture at 170° C. for 20 minutes; and
cooling the mixture so that a nonwoven fabric for test having a thickness of 10 mm and a basis weight of 480 g/m2 is obtained,
measuring a normal incidence transmission loss of the obtained nonwoven fabric for test at a frequency of 400 to 5,000 Hz; and
calculating an average of the normal incidence transmission loss.

### Claim 8

A method for manufacturing a modified cross-section fiber, comprising:
obtaining a fibrous substance by discharging of a fiber raw material from a discharge hole which has a discharge hole area of 100 to 3,000 μm2 and has a shape satisfying modified cross-section degree (α′) of 1.5 to 4.0 calculated by Equation (2); and
setting a single fiber fineness of the fibrous substance to be 0.01 to 1.0 dtex,
α′=P′/(4πA′)1/2 (2)
in the equation, P′ is a peripheral length (unit: μm) of the shape of the discharge hole, and A′ is the discharge hole area (unit: μm2).

### Claim 9 (depends on 1)

A nonwoven fabric comprising 10% by mass or more of the modified cross-section fiber according to claim 1.

### Claim 10 (depends on 9)

The nonwoven fabric according to claim 9 having a basis weight of 100 to 500 g/m2 and a thickness of 3 to 30 mm.

### Claim 11 (depends on 9)

The nonwoven fabric according to claim 9 having an average normal incidence transmission loss equal to or higher than 5.1 dB at a frequency of 400 to 5,000 Hz.

### Claim 12 (depends on 9)

The nonwoven fabric according to claim 9, comprising 10% to 90% by mass of the modified cross-section fiber and 10% to 40% by mass of a melting fiber, wherein a total content of the modified cross-section fiber and the melting fiber is 20% to 100% by mass.

### Claim 13 (depends on 1)

A noise-absorbing and -insulating material comprising 10% by mass or more of the modified cross-section fiber according to claim 1.

### Claim 14 (depends on 9)

A noise-absorbing and -insulating material comprising 50% by mass or more of the nonwoven fabric according to claim 9.

### Claim 15 (depends on 2)

The modified cross-section fiber according to claim 2, wherein the fiber cross section is Y-shaped, cross-shaped, 6-lobed, 8-lobed, or pinwheel-shaped.

### Claim 16 (depends on 2)

The modified cross-section fiber according to claim 2, which is a polyester fiber, a polypropylene fiber, a nylon fiber, an aramid fiber, an acrylic fiber, or a rayon fiber.

### Claim 17 (depends on 3)

The modified cross-section fiber according to claim 3, which is a polyester fiber, a polypropylene fiber, a nylon fiber, an aramid fiber, an acrylic fiber, or a rayon fiber.

### Claim 18 (depends on 2)

The modified cross-section fiber according to claim 2 having a noise absorption coefficient equal to or higher than 0.40 at a frequency of 400 to 1,250 Hz, wherein the noise absorption coefficient is measured in a noise-absorbing and -insulating performance test (I), the noise-absorbing and -insulating performance test (I) comprising:
cutting a fiber (0.81 g) in a length of 40 mm;
putting the cut fiber in a cylindrical holder having a diameter of 41.5 mm and a thickness of 30 mm;
measuring a normal incidence noise absorption coefficient at a frequency of 400 to 1,250 Hz; and
calculating an average of the coefficient.

### Claim 19 (depends on 2)

The modified cross-section fiber according to claim 2 having a noise absorption coefficient equal to or higher than 0.17 at a frequency of 400 to 1,250 Hz, wherein the noise absorption coefficient is measured in a noise-absorbing and -insulating performance test (II), the noise-absorbing and -insulating performance test (II) comprising:
cutting a fiber (0.27 g) in a length of 40 mm;
putting the cut fiber in a cylindrical holder having a diameter of 41.5 mm and a thickness of 20 mm;
measuring a normal incidence noise absorption coefficient at a frequency of 400 to 1,250 Hz; and
calculating an average of the coefficient.

### Claim 20 (depends on 2)

The modified cross-section fiber according to claim 2 having a transmission loss equal to or higher than 5.1 dB at a frequency of 400 to 5,000 Hz, wherein the transmission loss is measured in a noise-absorbing and -insulating performance test (III), the noise-absorbing and -insulating performance test (III) comprising:
mixing the modified cross-section fiber (70% by mass) having a fiber length of 40 mm with 30% by mass of a polyester melting fiber having a single fiber fineness of 2.2 dtex, a fiber length of 51 mm, and a melting point of 110° C.;
heating the mixture at 170° C. for 20 minutes; and
cooling the mixture so that a nonwoven fabric for test having a thickness of 10 mm and a basis weight of 480 g/m2 is obtained,
measuring a normal incidence transmission loss of the obtained nonwoven fabric for test at a frequency of 400 to 5,000 Hz; and
calculating an average of the normal incidence transmission loss.