# US 2021/0079503 A1 · Magnesium alloy sheet and method for producing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0079503 A1
- Document ID: US20210079503A1
- Status: Published application
- Kind: A1
- Application number: 16/954,377
- Filed: 2018-12-21
- Published: 2021-03-18
- Earliest claimed: 2017-12-26
- Assignees: Posco
- Applicants: Posco
- Inventors: Jun Ho Park; Hyun Bom Lee; Jae Joong Kim; Oh-Duck Kwon
- Web page: https://patentgrep.com/patent/US20210079503A1

## CPC

- C22C 23/02: with aluminium as the next major constituent
- B21B 3/003: {Rolling non-ferrous metals immediately subsequent to continuous casting, i.e. in-line rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C22C 23/04: with zinc or cadmium as the next major constituent
- C22F 1/06: of magnesium or alloys based thereon
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

The present invention relates to a magnesium alloy sheet and a manufacturing method thereof. In detail, the magnesium alloy sheet includes 0.5 to 3.5 wt % of Al, 0.5 to 1.5 wt % of Zn, 0.1 to 1.0 wt % of Ca, 0.01 to 1.0 wt % of Mn, a remainder of Mg, and other inevitable impurities with respect to an entire 100 wt % of a magnesium alloy sheet, wherein an average crystal grain size of the magnesium alloy sheet is 3 to 15 μm, the magnesium alloy sheet includes a stringer, and a length of the stringer in a rolling direction (RD) is equal to or less than the maximum value of 50 μm.

## Claims

### Claim 1

A magnesium alloy sheet comprising:
0.5 to 3.5 wt % of Al, 0.5 to 1.5 wt % of Zn, 0.1 to 1.0 wt % of Ca, 0.01 to 1.0 wt % of Mn, a remainder of Mg, and other inevitable impurities with respect to an entire 100 wt % of the magnesium alloy sheet,
wherein an average crystal grain size of the magnesium alloy sheet is 3 to 15 μm.

### Claim 2 (depends on 1)

The magnesium alloy sheet of claim 1, wherein
the magnesium alloy sheet includes a stringer, and
a length of the stringer in a rolling direction (RD) is equal to or less than a maximum value of 50 μm.

### Claim 3 (depends on 2)

The magnesium alloy sheet of claim 2, wherein
a thickness of the stringer in a transverse direction (TD) is equal to or less than a maximum value of 1 μm on the magnesium alloy sheet.

### Claim 4 (depends on 3)

The magnesium alloy sheet of claim 3, wherein
the magnesium alloy sheet has a limited bending radius (LBR) value in the rolling direction (RD) at equal to or greater than 150° C. that is equal to or less than 0.5 R/t.

### Claim 5 (depends on 4)

The magnesium alloy sheet of claim 4, wherein
the magnesium alloy sheet has a limited bending radius (LBR) value in the transverse direction (TD) at equal to or greater than 150° C. that is equal to or less than 1.5 R/t.

### Claim 6 (depends on 5)

The magnesium alloy sheet of claim 5, wherein
regarding the magnesium alloy sheet,
an absolute value of a difference between limited bending radius (LBR) values in the rolling direction (RD) and the transverse direction (TD) at equal to or greater than 150° C. is 0.4 to 1.4.

### Claim 7 (depends on 6)

The magnesium alloy sheet of claim 6, wherein
a thickness of the magnesium alloy sheet is 0.8 to 1.7 mm.

### Claim 8

A method for manufacturing a magnesium alloy sheet, comprising:
preparing a casting material by casting an alloy melt solution including 0.5 to 3.5 wt % of Al, 0.5 to 1.5 wt % of Zn, 0.1 to 1.0 wt % of Ca, 0.01 to 1.0 wt % of Mn, a remainder of Mg, and other inevitable impurities for the entire 100 wt %;
homogenizing and heat-treating the casting material;
preparing a rolled material by rolling the homogenized and heat-treated casting material; and
finally annealing the rolled material,
wherein, in the preparing of a rolled material,
a cumulative reduction ratio is equal to or greater than 86%.

### Claim 9 (depends on 8)

The method of claim 8, wherein
the homogenizing and heat-treating of a casting material is performed at a temperature of 300 to 500° C.

### Claim 10 (depends on 9)

The method of claim 9, wherein
the homogenizing and heat-treating of a casting material is performed for 4 to 30 hours.

### Claim 11 (depends on 8)

The method of claim 8, wherein
the homogenizing and heat-treating of a casting material includes:
a first homogenization and heat treatment; and
a secondary homogenization and heat treatment.

### Claim 12 (depends on 11)

The method of claim 11, wherein
the first homogenization and heat treatment is performed at a temperature of 300 to 400° C.

### Claim 13 (depends on 12)

The method of claim 12, wherein
the first homogenization and heat treatment is performed for 1 to 15 hours.

### Claim 14 (depends on 11)

The method of claim 11, wherein
the secondary homogenization and heat treatment is performed at a temperature of 400 to 500° C.

### Claim 15 (depends on 14)

The method of claim 14, wherein
the secondary homogenization and heat treatment is performed for 1 to 15 hours.

### Claim 16 (depends on 8)

The method of claim 8, wherein
the preparing of a rolled material is performed at a temperature of 200 to 400° C.

### Claim 17 (depends on 16)

The method of claim 16, wherein
the preparing of a rolled material includes performing rolling with a reduction ratio that is greater than 0 and equal to or less than 50% for each rolling.

### Claim 18 (depends on 8)

The method of claim 8, wherein
the preparing of a rolled material further includes
intermediately annealing the rolled material.

### Claim 19 (depends on 18)

The method of claim 18, wherein
the intermediately annealing of the rolled material is performed at a temperature of 300 to 500° C., wherein
the intermediately annealing of the rolled material is performed for 30 minutes to 10 hours.

### Claim 20

(canceled)

### Claim 21 (depends on 8)

The method of claim 8, wherein
the finally annealing of a rolled material is performed at a temperature of 300 to 500° C., wherein
the finally annealing of a rolled material is performed for 10 minutes to 10 hours.

### Claim 22

(canceled)