# US 2021/0062286 A1 · Non-oriented electrical steel sheet and method for manufacturing non-oriented electrical steel sheet

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0062286 A1
- Document ID: US20210062286A1
- Status: Published application
- Kind: A1
- Application number: 16/958,097
- Filed: 2019-02-15
- Published: 2021-03-04
- Earliest claimed: 2018-02-16
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Takeshi KUBOTA; Takeaki WAKISAKA; Masafumi MIYAZAKI; Takashi MOROHOSHI
- Web page: https://patentgrep.com/patent/US20210062286A1

## CPC

- C21D 9/46: for sheet metals
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/1222: {Hot rolling}
- C21D 8/1233: {Cold rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/16: containing copper
- H01F 1/147: Alloys characterised by their composition {(treatment thereof for enhancing their electromagnetic properties C21D8/12)}
- C22C 2202/02: Magnetic
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

A non-oriented electrical steel sheet according to one embodiment of the invention has a chemical composition represented by C: 0.0030% or less, Si: 2.00% or less, Al: 1.00% or less, Mn: 0.10% to 2.00%, S: 0.0030% or less, one or more selected from the group consisting of Mg, Ca, Sr, Ba, Nd, Pr, La, Ce, Zn, and Cd: 0.0003% or greater and less than 0.0015% in total, a parameter Q represented by Q=[Si]+2x[Al]−[Mn]: 2.00 or less; Sn: 0.00% to 0.40%, Cu: 0.00% to 1.00%, and a remainder: Fe and impurities, and a parameter R represented by R−(I100+I310+I411+I521)/(I111+I211+I332+I221) is 0.80 or greater.

## Claims

### Claim 1

A non-oriented electrical steel sheet comprising, as a chemical composition, by mass %:
C: 0.0030% or less;
Si: 2.00% or less;
Al: 1.00% or less;
Mn: 0.10% to 2.00%;
S: 0.0030% or less;
one or more selected from the group consisting of Mg, Ca, Sr, Ba, Nd, Pr, La, Ce, Zn, and Cd: 0.0003% or greater and less than 0.0015% in total;
a parameter Q represented by Formula 1 where [Si] denotes a Si content (mass %), [Al] denotes an Al content (mass %), and [Mn] denotes a Mn content (mass %) : 2.00 or less;
Sn: 0.00% to 0.40%;
Cu: 0.00% to 1.00%; and
a remainder: Fe and impurities,
wherein a parameter R represented by Formula 2 where I100, I130, I411, I521, I111, I211, I332, and I221 denote a {100} crystal orientation intensity, a {310} crystal orientation intensity, a {411} crystal orientation intensity, a {521} crystal orientation intensity, a {111} crystal orientation intensity, a {211} crystal orientation intensity, a {332} crystal orientation intensity, and a {221} crystal orientation intensity in a thickness middle portion, respectively, is 0.80 or greater
Q=[Si]+2×[Al]−[Mn] (Formula 1)
R=(I110+I310+I411+I521)/(I111+I211+I332+I221) (Formula 2).

### Claim 2 (depends on 1)

The non-oriented electrical steel sheet according to claim 1,
wherein in the chemical composition, either Sn: 0.02% to 0.40% or Cu: 0.10% to 1.00%, or both are satisfied.

### Claim 3 (depends on 1)

A method for manufacturing the non-oriented electrical steel sheet according to claim 1, comprising:
continuous casting a molten steel;
hot rolling a steel ingot obtained by the continuous casting;
cold rolling a steel strip obtained by the hot rolling; and
final annealing a cold rolled steel sheet obtained by the cold rolling,
wherein the molten steel has the chemical composition according to claim 1,
the steel strip has a columnar grain ratio of 80% or greater by area fraction and an average grain size of 0.10 mm or greater, and
a rolling reduction in the cold rolling is 90% or less.

### Claim 4 (depends on 3)

The method for manufacturing the non-oriented electrical steel sheet according to claim 3,
wherein in the continuous casting, a temperature difference between one surface and the other surface of the steel ingot during solidification is 40° C. or higher.

### Claim 5 (depends on 3)

The method for manufacturing the non-oriented electrical steel sheet according to claim 3,
wherein in the hot rolling, a hot rolling start temperature is 900° C. or lower, and a coiling temperature for the steel strip is 650° C. or lower.

### Claim 6 (depends on 3)

The method for manufacturing the non-oriented electrical steel sheet according to claim 3,
wherein in the final annealing, a sheet traveling tension is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 7 (depends on 1)

A method for manufacturing the non-oriented electrical steel sheet according to claim 1, comprising:
rapid solidifying a molten steel;
cold rolling a steel strip obtained by the rapid solidifying; and
final annealing a cold rolled steel sheet obtained by the cold rolling,
wherein the molten steel has the chemical composition according to claim 1,
the steel strip has a columnar grain ratio of 80% or greater by area fraction and an average grain size of 0.10 mm or greater, and
a rolling reduction in the cold rolling is 90% or less.

### Claim 8 (depends on 7)

The method for manufacturing the non-oriented electrical steel sheet according to claim 7,
wherein in the rapid solidifying, the molten steel is solidified by using a moving cooling wall, and
a temperature of the molten steel to be injected to the moving cooling wall is adjusted to be at least 25° C. higher than a solidification temperature of the molten steel.

### Claim 9 (depends on 7)

The method for manufacturing the non-oriented electrical steel sheet according to claim 7,
wherein in the rapid solidifying, the molten steel is solidified by using a moving cooling wall, and
an average cooling rate from completion of the solidification of the molten steel to coiling of the steel strip is 1,000 to 3,000° C./min.

### Claim 10 (depends on 7)

The method for manufacturing the non-oriented electrical steel sheet according to claim 7,
wherein a sheet traveling tension in the final annealing is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 11 (depends on 4)

The method for manufacturing the non-oriented electrical steel sheet according to claim 4,
wherein in the hot rolling, a hot rolling start temperature is 900° C. or lower, and a coiling temperature for the steel strip is 650° C. or lower.

### Claim 12 (depends on 4)

The method for manufacturing the non-oriented electrical steel sheet according to claim 4,
wherein in the final annealing, a sheet traveling tension is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 13 (depends on 5)

The method for manufacturing the non-oriented electrical steel sheet according to claim 5,
wherein in the final annealing, a sheet traveling tension is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 14 (depends on 11)

The method for manufacturing the non-oriented electrical steel sheet according to claim 11,
wherein in the final annealing, a sheet traveling tension is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 15 (depends on 8)

The method for manufacturing the non-oriented electrical steel sheet according to claim 8,
wherein in the rapid solidifying, the molten steel is solidified by using a moving cooling wall, and
an average cooling rate from completion of the solidification of the molten steel to coiling of the steel strip is 1,000 to 3,000° C./min.

### Claim 16 (depends on 8)

The method for manufacturing the non-oriented electrical steel sheet according to claim 8,
wherein a sheet traveling tension in the final annealing is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 17 (depends on 9)

The method for manufacturing the non-oriented electrical steel sheet according to claim 9,
wherein a sheet traveling tension in the final annealing is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 18 (depends on 15)

The method for manufacturing the non-oriented electrical steel sheet according to claim 15,
wherein a sheet traveling tension in the final annealing is 3 MPa or less, and a cooling rate from 950° C. to 700° C. is 1° C./sec or less.

### Claim 19 (depends on 2)

A method for manufacturing the non-oriented electrical steel sheet according to claim 2, comprising:
continuous casting a molten steel;
hot rolling a steel ingot obtained by the continuous casting;
cold rolling a steel strip obtained by the hot rolling; and
final annealing a cold rolled steel sheet obtained by the cold rolling,
wherein the molten steel has the chemical composition according to claim 2,
the steel strip has a columnar grain ratio of 80% or greater by area fraction and an average grain size of 0.10 mm or greater, and
a rolling reduction in the cold rolling is 90% or less.

### Claim 20 (depends on 2)

A method for manufacturing the non-oriented electrical steel sheet according to claim 2, comprising:
rapid solidifying a molten steel;
cold rolling a steel strip obtained by the rapid solidifying; and
final annealing a cold rolled steel sheet obtained by the cold rolling,
wherein the molten steel has the chemical composition according to claim 2,
the steel strip has a columnar grain ratio of 80% or greater by area fraction and an average grain size of 0.10 mm or greater, and
a rolling reduction in the cold rolling is 90% or less.