# US 2021/0062282 A1 · High-strength steel sheet and method for producing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0062282 A1
- Document ID: US20210062282A1
- Status: Published application
- Kind: A1
- Application number: 16/957,739
- Filed: 2018-10-09
- Published: 2021-03-04
- Earliest claimed: 2017-12-27
- Assignees: Jfe Steel Corporation
- Applicants: JFE Steel Corporation
- Inventors: Hiroshi Hasegawa; Hidekazu Minami; Tatsuya Nakagaito; Kana Sasaki; Shoji Tanaka
- Web page: https://patentgrep.com/patent/US20210062282A1

## CPC

- C21D 9/46: for sheet metals
- C21D 6/005: {containing Mn}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/26: with niobium or tantalum
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/29: {Cooling or quenching}
- C23C 2/40: Plates; Strips
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A high-strength steel sheet has a specific composition and a microstructure. In the microstructure, the area fraction of elongated ferrite phase grains having an aspect ratio of 3 or more is 1% or less, the average crystal grain size of martensite included in a region extending 50 μm from a surface of the steel sheet is 20 μm or less, the content of oxide particles having a minor axis length of 0.8 μm or less in the region extending 50 μm from the surface of the steel sheet is 1.0×1010 particles/m2 or more, and the content of coarse oxide particles having a minor axis length of more than 1 μm in the region extending 50 μm from the surface of the steel sheet is 1.0×108 particles/m2 or less. The content of hydrogen trapped in the steel sheet is 0.05 ppm by mass or more.

## Claims

### Claim 1

A high-strength steel sheet comprising:
a composition containing, by mass,
C: 0.05% to 0.40%,
Si: 0.10% to 3.0%,
Mn: 1.5% to 4.0%,
P: 0.100% or less (excluding 0%),
S: 0.02% or less (excluding 0%),
Al: 0.010% to 1.0%, and
N: 0.010% or less, with the balance being Fe and inevitable impurities;
a microstructure including lower bainite, martensite, retained austenite, upper bainite, and ferrite such that the total area fraction of the lower bainite, the martensite, and the retained austenite is 40% to 100%, the area fraction of the retained austenite is 15% or less, and the total area fraction of the upper bainite and the ferrite is 0% to 60%,
wherein, in the microstructure, the area fraction of elongated ferrite phase grains having an aspect ratio of 3 or more is 1% or less, the average crystal grain size of martensite included in a region extending 50 μm from a surface of the steel sheet is 20 μm or less, the content of oxide particles having a minor axis length of 0.8 μm or less in the region extending 50 μm from the surface of the steel sheet is 1.0×1010 particles/m2 or more, and the content of coarse oxide particles having a minor axis length of more than 1.0 μm in the region extending 50 μm from the surface of the steel sheet is 1.0×108 particles/m2 or less; and
a content of hydrogen trapped in the steel sheet is 0.05 ppm by mass or more.

### Claim 2 (depends on 1)

The high-strength steel sheet according to claim 1, further comprising one or more elements selected from, by mass:
Cr: 0.005% to 2.0%,
Ti: 0.005% to 0.20%,
Nb: 0.005% to 0.20%,
Mo: 0.005% to 2.0%,
V: 0.005% to 2.0%,
Ni: 0.005% to 2.0%,
Cu: 0.005% to 2.0%,
B: 0.0001% to 0.0050%,
Ca: 0.0001% to 0.0050%,
REM: 0.0001% to 0.0050%,
Sn: 0.01% to 0.50%, and
Sb: 0.0010% to 0.10%.

### Claim 3 (depends on 1)

The high-strength steel sheet according to claim 1, comprising a coating film constituted by one or more layers, the coating film being disposed on the surface of the steel sheet.

### Claim 4 (depends on 2)

The high-strength steel sheet according to claim 2, comprising a coating film constituted by one or more layers, the coating film being disposed on the surface of the steel sheet.

### Claim 5 (depends on 1)

The high-strength steel sheet according to claim 1, comprising a galvanizing layer disposed on the surface of the steel sheet.

### Claim 6 (depends on 2)

The high-strength steel sheet according to claim 2, comprising a galvanizing layer disposed on the surface of the steel sheet.

### Claim 7 (depends on 1)

The high-strength steel sheet according to claim 1, comprising an alloyed hot-dip galvanizing layer disposed on the surface of the steel sheet.

### Claim 8 (depends on 2)

The high-strength steel sheet according to claim 2, comprising an alloyed hot-dip galvanizing layer disposed on the surface of the steel sheet.

### Claim 9 (depends on 1)

A method for producing a high-strength steel sheet, the method comprising:
a hot-rolling step of rough-rolling a slab having the composition according to claim 1, subsequently performing descaling at a pressure of 15 MPa or more, then performing finish rolling at 800° C. to 950° C., performing cooling subsequent to the finish rolling, and then performing coiling at 550° C. or less;
an annealing step of heating a hot-rolled steel sheet produced in the hot-rolling step to 730° C. to 950° C. and performing holding at 730° C. to 950° C. in an atmosphere having a hydrogen concentration of 1.0% to 35.0% by volume and a dew point of −35° C. to 15° C. for 10 to 1000 s;
a cooling step of cooling a steel sheet treated in the annealing step to 600° C. at an average rate of 5° C./s or more, stopping the cooling at a temperature of more than Ms and 600° C. or less, subsequently performing retention at a temperature of more than Ms and 600° C. or less for 1000 s or less, and, subsequent to the retention, performing cooling to room temperature such that the average cooling rate between Ms and 50° C. is 1.0° C./s or more;
an elongation rolling step of rolling a steel sheet treated in the cooling step at an elongation ratio of 0.05% to 1%; and
an aging treatment step of subjecting a steel sheet treated in the elongation rolling step to an aging treatment under conditions satisfying Formula (1) below,
(273+T)×(20+log10(t))≥6800, (1)
where T is a temperature (° C.) of 200° C. or less, and t is a time (hr).

### Claim 10 (depends on 2)

A method for producing a high-strength steel sheet, the method comprising:
a hot-rolling step of rough-rolling a slab having the composition according to claim 2, subsequently performing descaling at a pressure of 15 MPa or more, then performing finish rolling at 800° C. to 950° C., performing cooling subsequent to the finish rolling, and then performing coiling at 550° C. or less;
an annealing step of heating a hot-rolled steel sheet produced in the hot-rolling step to 730° C. to 950° C. and performing holding at 730° C. to 950° C. in an atmosphere having a hydrogen concentration of 1.0% to 35.0% by volume and a dew point of −35° C. to 15° C. for 10 to 1000 s;
a cooling step of cooling a steel sheet treated in the annealing step to 600° C. at an average rate of 5° C./s or more, stopping the cooling at a temperature of more than Ms and 600° C. or less, subsequently performing retention at a temperature of more than Ms and 600° C. or less for 1000 s or less, and, subsequent to the retention, performing cooling to room temperature such that the average cooling rate between Ms and 50° C. is 1.0° C./s or more;
an elongation rolling step of rolling a steel sheet treated in the cooling step at an elongation ratio of 0.05% to 1%; and an aging treatment step of subjecting a steel sheet treated in the elongation rolling step to an aging treatment under conditions satisfying Formula (1) below,
(273+T)×(20+log10(t))≥6800, (1)
where T is a temperature (° C.) of 200° C. or less, and t is a time (hr).

### Claim 11 (depends on 1)

A method for producing a high-strength steel sheet, the method comprising:
a hot-rolling step of rough-rolling a slab having the composition according to claim 1, subsequently performing descaling at a pressure of 15 MPa or more, then performing finish rolling at 800° C. to 950° C., performing cooling subsequent to the finish rolling, and then performing coiling at 550° C. or less;
a cold-rolling step of cold-rolling a hot-rolled steel sheet produced in the hot-rolling step at a rolling reduction ratio of 20% or more;
an annealing step of heating a cold-rolled steel sheet produced in the cold-rolling step to 730° C. to 950° C. and performing holding at 730° C. to 950° C. in an atmosphere having a hydrogen concentration of 1.0% to 35.0% by volume and a dew point of −35° C. to 15° C. for 10 to 1000 s;
a cooling step of cooling a steel sheet treated in the annealing step to 600° C. at an average rate of 5° C./s or more, stopping the cooling at a temperature of more than Ms and 600° C. or less, subsequently performing retention at a temperature of more than Ms and 600° C. or less for 1000 s or less, and, subsequent to the retention, performing cooling to room temperature such that the average cooling rate between Ms and 50° C. is 1.0° C./s or more;
an elongation rolling step of rolling a steel sheet treated in the cooling step at an elongation ratio of 0.05% to 1%; and
an aging treatment step of subjecting a steel sheet treated in the elongation rolling step to an aging treatment under conditions satisfying Formula (1) below,
(273+T)×(20+log10(t))≥6800, (1)
where T is a temperature (° C.) of 200° C. or less, and t is a time (hr).

### Claim 12 (depends on 2)

A method for producing a high-strength steel sheet, the method comprising:
a hot-rolling step of rough-rolling a slab having the composition according to claim 2, subsequently performing descaling at a pressure of 15 MPa or more, then performing finish rolling at 800° C. to 950° C., performing cooling subsequent to the finish rolling, and then performing coiling at 550° C. or less;
a cold-rolling step of cold-rolling a hot-rolled steel sheet produced in the hot-rolling step at a rolling reduction ratio of 20% or more;
an annealing step of heating a cold-rolled steel sheet produced in the cold-rolling step to 730° C. to 950° C. and performing holding at 730° C. to 950° C. in an atmosphere having a hydrogen concentration of 1.0% to 35.0% by volume and a dew point of −35° C. to 15° C. for 10 to 1000 s;
a cooling step of cooling a steel sheet treated in the annealing step to 600° C. at an average rate of 5° C./s or more, stopping the cooling at a temperature of more than Ms and 600° C. or less, subsequently performing retention at a temperature of more than Ms and 600° C. or less for 1000 s or less, and, subsequent to the retention, performing cooling to room temperature such that the average cooling rate between Ms and 50° C. is 1.0° C./s or more;
an elongation rolling step of rolling a steel sheet treated in the cooling step at an elongation ratio of 0.05% to 1%; and
an aging treatment step of subjecting a steel sheet treated in the elongation rolling step to an aging treatment under conditions satisfying Formula (1) below,
(273+T)×(20+log10(t))≥6800, (1)
where T is a temperature (° C.) of 200° C. or less, and t is a time (hr).

### Claim 13 (depends on 9)

The method for producing a high-strength steel sheet according to claim 9, wherein a coating film formation treatment is performed in any of the steps subsequent to the annealing step.

### Claim 14 (depends on 10)

The method for producing a high-strength steel sheet according to claim 10, wherein a coating film formation treatment is performed in any of the steps subsequent to the annealing step.

### Claim 15 (depends on 11)

The method for producing a high-strength steel sheet according to claim 11, wherein a coating film formation treatment is performed in any of the steps subsequent to the annealing step.

### Claim 16 (depends on 12)

The method for producing a high-strength steel sheet according to claim 12, wherein a coating film formation treatment is performed in any of the steps subsequent to the annealing step.

### Claim 17 (depends on 9)

The method for producing a high-strength steel sheet according to claim 9, wherein a galvanizing treatment is performed in the cooling step.

### Claim 18 (depends on 10)

The method for producing a high-strength steel sheet according to claim 10, wherein a galvanizing treatment is performed in the cooling step.

### Claim 19 (depends on 11)

The method for producing a high-strength steel sheet according to claim 11, wherein a galvanizing treatment is performed in the cooling step.

### Claim 20 (depends on 12)

The method for producing a high-strength steel sheet according to claim 12, wherein a galvanizing treatment is performed in the cooling step.

### Claim 21 (depends on 17)

The method for producing a high-strength steel sheet according to claim 17, wherein an alloying treatment is further performed subsequent to the galvanizing treatment.

### Claim 22 (depends on 18)

The method for producing a high-strength steel sheet according to claim 18, wherein an alloying treatment is further performed subsequent to the galvanizing treatment.

### Claim 23 (depends on 19)

The method for producing a high-strength steel sheet according to claim 19, wherein an alloying treatment is further performed subsequent to the galvanizing treatment.

### Claim 24 (depends on 20)

The method for producing a high-strength steel sheet according to claim 20, wherein an alloying treatment is further performed subsequent to the galvanizing treatment.