# US 2020/0395830 A1 · Radially oriented solid cylindrical magnet and production method and device thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0395830 A1
- Document ID: US20200395830A1
- Status: Published application
- Kind: A1
- Application number: 16/888,060
- Filed: 2020-05-29
- Published: 2020-12-17
- Earliest claimed: 2019-06-11
- Assignees: Shenzhen Radimag Magnets Co., Ltd
- Applicants: Shenzhen Radimag Magnets Co.,Ltd
- Inventors: Wenhao CHENG
- Web page: https://patentgrep.com/patent/US20200395830A1

## CPC

- H02K 15/03: having permanent magnets
- B22F 3/12: Both compacting and sintering (by forging B22F3/17)
- B22F 3/16: in successive or repeated steps
- H02K 1/02: characterised by the magnetic material
- H02K 1/2726: the rotor consisting of a single magnet or two or more axially juxtaposed single magnets
- H02K 1/2733: Annular magnets
- H02K 1/30: using intermediate parts, e.g. spiders
- H02K 2213/03: Machines characterised by numerical values, ranges, mathematical expressions or similar information
- H02K: DYNAMO-ELECTRIC MACHINES (dynamo-electric relays H01H53/00; conversion of DC or AC input power into surge output power {H03K3/53})
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER

## Abstract

The present disclosure provides a radially oriented solid cylindrical magnet, a method and device for molding and manufacturing the same, and a rotor and motor component using the same. The radial orientation degree of the solid cylindrical magnet is greater than or equal to 90%. A mold includes no mold core. Magnetic particles in the mold are continuously rotated in a magnetic field during molding, and an oriented magnetic field is applied during molding. The manufactured solid cylindrical magnet can be directly used as a rotor of a micro-motor to replace a conventional rotor with a radially oriented magnet ring, or can be used for producing radially oriented magnet rings with an arbitrary inner diameter, so as to obtain radially oriented magnet rings having an inner diameter less than 3 mm or even less for micro-motors.

## Claims

### Claim 1

A method for molding a radially oriented solid cylindrical magnet, wherein the radial orientation degree of the solid cylindrical magnet is greater than or equal to 90%; and, the diameter D of the solid cylindrical magnet and the width W of an oriented magnetic field satisfy the following relationship: W=nD+W0, where n is 0.05 to 5, W0 is 0.1 to 1, and the width W of the oriented magnetic field is the width of a parallel magnetic field in the center of poles for the oriented magnetic field.

### Claim 2 (depends on 1)

The method for molding a radially oriented solid cylindrical magnet according to claim 1, wherein a mold without a mold core; a quasi-2D oriented magnetic field is applied during molding, and magnetic particles in a mold cavity are continuously rotated in the magnetic field during molding; preferably, the magnetic particles are anisotropic; and more preferably, a magnetic field that changes by stages is applied during molding, comprising: a first magnetic field applied to fully magnetize the magnetic particles in the mold cavity, a second magnetic field applied to enable the fully-magnetized magnetic particles in the mold cavity to continuously rotate in the quasi-2D oriented magnetic field, a third magnetic field applied when the density of a blank in the mold cavity reaches a level at which the magnetic particles cannot be rotated freely after leaving the oriented magnetic field, and a fourth magnetic field applied to enable the blank in the mold cavity to have a desired density, with the intensity of the first magnetic field being 1 to 3 times of that of the second magnetic field, the intensity of the third magnetic field being 1 to 0 times of that of the second magnetic field and the intensity of the fourth magnetic field being 0.5 to 0.01 times that of the second magnetic field.

### Claim 3

A method for molding a radially oriented solid cylindrical magnet, comprising following steps of:
(1) preparing a mold without a mold core;
(2) mounting the prepared mold in a magnetic field generation device perpendicular to a cylindrical surface of the mold, the magnetic field generation device preferably comprising at least two outer poles arranged symmetrically, and the width of a parallel magnetic field in the center of the two outer poles being the width of an oriented magnetic field; and applying a quasi-2D oriented magnetic field during molding, wherein the mold comprises a mold sleeve, a mold cavity, an upper ram and a lower ram;
(3) filling anisotropic magnetic particles in the mold cavity;
(4) applying a first magnetic field and then continuously rotating the mold and the magnetic particles in the mold cavity; or, continuously rotating the mold and the magnetic particles in the mold cavity and then applying a first magnetic field;
(5) applying a second magnetic field, continuously rotating the mold and the magnetic particles in the mold cavity, applying an increased stress to the magnetic particles in the mold cavity by both the upper and lower rams, and maintaining this stress for a certain period of time to obtain a blank; or, by keeping the lower ram unmoved, moving the upper ram down to apply an increased stress to the magnetic particles in the mold cavity and maintaining this stress for a certain period of time; or, by keeping the upper ram unmoved, moving the lower ram up to apply an increased stress to the magnetic particles in the mold cavity and maintaining this stress for a certain period of time, the certain period of time being the time required for the mold to rotate in at least one circle, and the stress being preferably 5 MPa to 200 MPa;
(6) when the density of the blank in the mold cavity reaches a level at which the magnetic particles cannot be rotated freely after leaving the oriented magnetic field, applying a third magnetic field, and continuously applying a stress by the rams until the blank has a desired density;
(7) after the blank in the mold cavity has a desired density, applying a fourth magnetic field to demagnetize the blank; and preferably, applying a reverse magnetic field to the blank in the mold cavity to demagnetize the blank, or applying a forward/reverse alternating magnetic field to demagnetize the blank in the mold cavity; and
(8) stopping the application of stress, stopping the rotation of the mold, and demolding to obtain the blank.

### Claim 4 (depends on 3)

The method according to claim 3, wherein, after the step (3), the upper ram of the mold is moved to a position in the mold cavity at the same height as upper edge of poles for the oriented magnetic field or a position slightly lower than upper edge of poles for the oriented magnetic field.

### Claim 5 (depends on 3)

The method according to claim 3, wherein, in the step (4), the magnetic field generation device firstly applies the first magnetic field to fully magnetize the magnetic particles in the mold cavity, and then applies the second magnetic field when the fully-magnetized magnetic particles in the mold cavity are continuously rotated in the quasi-2D oriented magnetic field, the intensity of the first magnetic field being 1 to 3 times of that of the second magnetic field; in the step (5), a gradually increased stress is applied to the magnetic particles during continuous rotation until the stress is increased to a certain level, and the magnetic particles in the mold cavity are always in the quasi-2D oriented magnetic field during the application of the gradually increased stress; in the step (6), the intensity of the applied third magnetic field is 1 to 0 times of that of the second magnetic field; and, in the step (7), after the blank in the mold cavity has a desired density, the intensity of the applied fourth magnetic field is 0.5 to 0.01 times of that of the second magnetic field.

### Claim 6 (depends on 2)

A method for radially oriented solid cylindrical sintered magnet, comprising steps of:
(1) molding a blank by the method according to claim 2; and
(2) sintering and aging, preferably including specific steps of:
(i) vacuumizing, in advance, to below 10−2 Pa;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1120° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 7 (depends on 2)

A method for radially oriented solid cylindrical bonded magnet, comprising steps of:
(1) molding a blank by the method according to claim 2; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 8 (depends on 2)

A molding device using the method according to claim 2, comprising a mold a magnetic field generation device, a rotating device and a device for applying stress by upper and lower rams;
the mold comprises a mold sleeve, a mold cavity, an upper ram and a lower ram, without a mold core;
the magnetic field generation device provides an oriented magnetic field discontinuously distributed around the sleeve within 360°, and comprises at least two outer poles arranged symmetrically; and
the rotating device drives the mold and magnetic particles in the mold cavity to continuously rotate in the magnetic field while the magnetic field generation device is kept unmoved, or drives the magnetic field generation device to rotate while the mold is kept unmoved, or drives both the mold and the magnetic field generation device to rotate simultaneously at different speeds.

### Claim 9 (depends on 6)

A micro-motor rotor, wherein the radially oriented solid cylindrical magnet manufactured by the method according to claim 6 is directly used as a micro-motor rotor.

### Claim 10 (depends on 6)

A component for a motor, wherein the radially oriented solid cylindrical magnet manufactured by the method according to claim 6 is mounted, as a permanent magnetic component for the motor, on a motor shaft by forming a hole with a desired inner diameter in the center of the magnet.

### Claim 11 (depends on 4)

The method according to claim 4, wherein, in the step (4), the magnetic field generation device firstly applies the first magnetic field to fully magnetize the magnetic particles in the mold cavity, and then applies the second magnetic field when the fully-magnetized magnetic particles in the mold cavity are continuously rotated in the quasi-2D oriented magnetic field, the intensity of the first magnetic field being 1 to 3 times of that of the second magnetic field; in the step (5), a gradually increased stress is applied to the magnetic particles during continuous rotation until the stress is increased to a certain level, and the magnetic particles in the mold cavity are always in the quasi-2D oriented magnetic field during the application of the gradually increased stress; in the step (6), the intensity of the applied third magnetic field is 1 to 0 times of that of the second magnetic field; and, in the step (7), after the blank in the mold cavity has a desired density, the intensity of the applied fourth magnetic field is 0.5 to 0.01 times of that of the second magnetic field.

### Claim 12 (depends on 3)

A method for radially oriented solid cylindrical sintered magnet, comprising steps of:
(1) molding a blank by the method according to claims 3; and
(2) sintering and aging, preferably including specific steps of:
(i) vacuumizing, in advance, to below 10−2 Pa;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1120° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 13 (depends on 4)

A method for radially oriented solid cylindrical sintered magnet, comprising steps of:
(1) molding a blank by the method according to claims 4; and
(2) sintering and aging, preferably including specific steps of:
(i) vacuumizing, in advance, to below 10−2 Pa;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1120° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 14 (depends on 5)

A method for radially oriented solid cylindrical sintered magnet, comprising steps of:
(1) molding a blank by the method according to claims 5; and
(2) sintering and aging, preferably including specific steps of:
(i) vacuumizing, in advance, to below 10−2 Pa;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1120° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 15 (depends on 11)

A method for radially oriented solid cylindrical sintered magnet, comprising steps of:
(1) molding a blank by the method according to claims 11; and
(2) sintering and aging, preferably including specific steps of:
(i) vacuumizing, in advance, to below 10−2 Pa;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1120° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 16 (depends on 3)

A method for radially oriented solid cylindrical bonded magnet, comprising steps of:
(1) molding a blank by the method according to claims 3; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 17 (depends on 4)

A method for radially oriented solid cylindrical bonded magnet, comprising steps of:
(1) molding a blank by the method according to claims 4; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 18 (depends on 5)

A method for radially oriented solid cylindrical bonded magnet, comprising steps of:
(1) molding a blank by the method according to claims 5; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 19 (depends on 11)

A method for radially oriented solid cylindrical bonded magnet, comprising steps of:
(1) molding a blank by the method according to claims 11; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 20 (depends on 3)

A molding device using the method according to claim 3, comprising a mold a magnetic field generation device, a rotating device and a device for applying stress by upper and lower rams;
the mold comprises a mold sleeve, a mold cavity, an upper ram and a lower ram, without a mold core;
the magnetic field generation device provides an oriented magnetic field discontinuously distributed around the sleeve within 360°, and comprises at least two outer poles arranged symmetrically; and
the rotating device drives the mold and magnetic particles in the mold cavity to continuously rotate in the magnetic field while the magnetic field generation device is kept unmoved, or drives the magnetic field generation device to rotate while the mold is kept unmoved, or drives both the mold and the magnetic field generation device to rotate simultaneously at different speeds.