# US 2020/0395828 A1 · Radially anisotropic multipolar solid magnet, and production method and device thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0395828 A1
- Document ID: US20200395828A1
- Status: Published application
- Kind: A1
- Application number: 16/887,976
- Filed: 2020-05-29
- Published: 2020-12-17
- Earliest claimed: 2019-06-11
- Assignees: Shenzhen Radimag Magnets Co., Ltd
- Applicants: Shenzhen Radimag Magnets Co.,Ltd
- Inventors: Wenhao CHENG
- Web page: https://patentgrep.com/patent/US20200395828A1

## CPC

- H02K 1/2733: Annular magnets
- H02K 15/03: having permanent magnets
- H02K 1/02: characterised by the magnetic material
- H02K 1/2726: the rotor consisting of a single magnet or two or more axially juxtaposed single magnets
- H02K 1/30: using intermediate parts, e.g. spiders
- H02K 2213/03: Machines characterised by numerical values, ranges, mathematical expressions or similar information
- H02K: DYNAMO-ELECTRIC MACHINES (dynamo-electric relays H01H53/00; conversion of DC or AC input power into surge output power {H03K3/53})

## Abstract

The present disclosure provides a molding method, a manufacturing method and a molding device for a radially anisotropic multipolar solid magnet, a micro-motor rotor using this magnet, and a component for a motor. A mold core is removed from a mold, and oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, are arranged outside the mold. The sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve. The magnet production method breaks through the dimensional restriction to the manufacturing of radially anisotropic multipolar magnets in the prior art, and can produce radially anisotropic multipolar magnets having an inner diameter or diameter less than 3 mm or even less for high-precision micro-motors.

## Claims

### Claim 1

A method for molding a radially anisotropic multipolar solid cylindrical magnet, wherein a mold core is removed from a mold; outer oriented poles, the number of which is the same as that of poles of the radially anisotropic multipolar solid cylindrical magnet, are arranged outside the mold; during and after the application of a magnetic field to magnetic particles, the mold and magnetic particles in a mold cavity are not required to rotate in the magnetic field, and oriented magnetic field is also not required to rotate; the sum L of widths or arc lengths of top ends of all the outer oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the mold comprises a mold cavity, an upper ram and a lower ram; an oriented magnetic field generation device comprises an even number (≥2) of symmetrical outer poles arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the outer oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of the mold sleeve.

### Claim 3

A method for molding a radially anisotropic multipolar solid cylindrical magnet, comprising following steps of:
(1) preparing a mold without a mold core;
(2) arranging, around the prepared mold, oriented poles, the number of which is the same as that of poles of the radially anisotropic multipolar solid cylindrical magnet, the sum L of widths or arc lengths of top ends of all the outer oriented poles being greater than or equal to 0.9πD, where L is the sum of widths or arc lengths of top ends of all the outer oriented poles and D is the outer diameter of a mold sleeve; filling anisotropic magnetic particles in a mold cavity, and moving an upper ram of the mold to a proper position, this position being preferably a position at the same height as an upper edge of poles for an oriented magnetic field or a position slightly lower than the upper edge of the poles for the oriented magnetic field;
(3) applying a first magnetic field to fully magnetize magnetic particles in the mold cavity;
(4) applying a second magnetic field, applying an increased stress to the magnetic particles in the mold cavity by both the upper and lower rams and maintaining this stress for a certain period of time to obtain a blank; or, by keeping the lower ram unmoved, moving the upper ram down to apply an increased stress to the magnetic particles in the mold cavity and maintaining this stress for a certain period of time, the stress being preferably 20 MPa to 200 MPa, preferably 50 MPa to 150 MPa;
(5) In the step (4), when the magnetic particles cannot recover to an out-of-order state before orientation after leaving the oriented magnetic field, applying a third magnetic field, and continuously applying a stress by the rams until the blank has a desired density;
(6) applying a fourth magnetic field to demagnetize the blank; and preferably, applying a reverse magnetic field to the blank in the mold cavity to demagnetize the blank, or applying a forward/reverse alternating magnetic field to demagnetize the blank in the mold cavity; and
(7) stopping the application of stress, and demolding to obtain the blank.

### Claim 4 (depends on 3)

The method according to claim 3, wherein, in the step (4), the intensity of the applied second magnetic field is lower than that of the first magnetic field, the intensity of the first magnetic field being 1 to 3 times but excluding 1 times of that of the second magnetic field; in the step (5), the intensity of the applied third magnetic field is 1 to 0 times of that of the second magnetic field; and, in the step (6), the applied four magnetic field is a reverse magnetic field or forward/reverse alternating magnetic field having an intensity that is 0.5 to 0.01 times of that of the second magnetic field.

### Claim 5 (depends on 2)

A method for manufacturing a radially anisotropic multipolar solid cylindrical magnet, comprising steps of:
(1) molding a magnet blank by the method according to claim 2; and
(2) sintering and aging, preferably comprising specific steps of:
(i) vacuumizing in advance;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1150° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 6 (depends on 2)

A method for manufacturing a radially anisotropic multipolar solid cylindrical magnet, comprising steps of:
(1) molding a magnet blank by the method according to claim 2; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 7 (depends on 1)

A molding device using the method according to claim 1, comprising a mold, an oriented magnetic field generation device and a stress applying device, wherein the mold comprises a mold cavity, an upper ram and a lower ram, without a mold core; the oriented magnetic field generation device comprises oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 8 (depends on 1)

A radially anisotropic multipolar solid cylindrical magnet manufactured by the method according to claim 1, wherein the inner diameter or diameter of the multipolar solid cylindrical magnet is less than 3 mm, and the orientation degree of the magnet is greater than or equal to 90%.

### Claim 9 (depends on 8)

A micro-motor rotor, wherein the micro-motor rotor directly uses the radially anisotropic multipolar solid cylindrical magnet according to claim 8.

### Claim 10 (depends on 8)

A component for a motor, wherein the radially anisotropic multipolar solid cylindrical magnet according to claim 8 is mounted, as a permanent magnetic component for the motor, on a motor shaft by forming a hole with a desired inner diameter in the center of the magnet.

### Claim 11 (depends on 3)

A method for manufacturing a radially anisotropic multipolar solid cylindrical magnet, comprising steps of:
(1) molding a magnet blank by the method according to claim 3; and
(2) sintering and aging, preferably comprising specific steps of:
(i) vacuumizing in advance;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1150° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 12 (depends on 4)

A method for manufacturing a radially anisotropic multipolar solid cylindrical magnet, comprising steps of:
(1) molding a magnet blank by the method according to claim 4; and
(2) sintering and aging, preferably comprising specific steps of:
(i) vacuumizing in advance;
(ii) heating, while vacuumizing, to a sintering temperature of 1000° C. to 1150° C.;
(iii) sintering in vacuum and maintaining the temperature;
(iv) feeding an inert gas and cooling; and
(vi) aging at 400° C. to 600° C., or aging at about 850° C. to 950° C. and then aging at 400° C. to 600° C.

### Claim 13 (depends on 3)

A method for manufacturing a radially anisotropic multipolar solid cylindrical magnet, comprising steps of:
(1) molding a magnet blank by the method according to claim 3; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 14 (depends on 4)

A method for manufacturing a radially anisotropic multipolar solid cylindrical magnet, comprising steps of:
(1) molding a magnet blank by the method according to claim 4; and
(2) heat treating to solidify an adhesive in the bonded magnet.

### Claim 15 (depends on 2)

A molding device using the method according to claim 2, comprising a mold, an oriented magnetic field generation device and a stress applying device, wherein the mold comprises a mold cavity, an upper ram and a lower ram, without a mold core; the oriented magnetic field generation device comprises oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 16 (depends on 3)

A molding device using the method according to claim 3, comprising a mold, an oriented magnetic field generation device and a stress applying device, wherein the mold comprises a mold cavity, an upper ram and a lower ram, without a mold core; the oriented magnetic field generation device comprises oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 17 (depends on 4)

A molding device using the method according to claim 4, comprising a mold, an oriented magnetic field generation device and a stress applying device, wherein the mold comprises a mold cavity, an upper ram and a lower ram, without a mold core; the oriented magnetic field generation device comprises oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 18 (depends on 5)

A molding device using the method according to claim 5, comprising a mold, an oriented magnetic field generation device and a stress applying device, wherein the mold comprises a mold cavity, an upper ram and a lower ram, without a mold core; the oriented magnetic field generation device comprises oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 19 (depends on 6)

A molding device using the method according to claim 6, comprising a mold, an oriented magnetic field generation device and a stress applying device, wherein the mold comprises a mold cavity, an upper ram and a lower ram, without a mold core; the oriented magnetic field generation device comprises oriented poles, the number of which is the same as that of poles of a radially anisotropic multipolar solid cylindrical magnet, arranged outside the mold; and, the sum L of widths or arc lengths of top ends of all the oriented poles is greater than or equal to 0.9πD, where D is the outer diameter of a mold sleeve.

### Claim 20 (depends on 2)

A radially anisotropic multipolar solid cylindrical magnet manufactured by the method according to claim 2, wherein the inner diameter or diameter of the multipolar solid cylindrical magnet is less than 3 mm, and the orientation degree of the magnet is greater than or equal to 90%.