# US 2020/0392608 A1 · Steel material for low yield ratio, high-strength steel pipe having excellent low-temperature toughness, and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0392608 A1
- Document ID: US20200392608A1
- Status: Published application
- Kind: A1
- Application number: 16/957,136
- Filed: 2018-12-18
- Published: 2020-12-17
- Earliest claimed: 2017-12-24
- Assignees: Posco
- Applicants: Posco
- Inventors: Jin-Ho BAE
- Web page: https://patentgrep.com/patent/US20200392608A1

## CPC

- C22C 38/02: containing silicon
- C22C 38/44: with molybdenum or tungsten
- C21D 6/00: Heat treatment of ferrous alloys
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/02: Hardening by precipitation
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 9/0081: {for slabs; for billets}
- C21D 9/46: for sheet metals
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/58: with more than 1.5% by weight of manganese
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/008: Martensite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A steel material for a low yield ratio, high-strength steel pipe having excellent low-temperature toughness according to an aspect of the present invention comprises, by weight %, 0.03-0.065% of C, 0.05-0.3% of Si, 1.7-2.2% of Mn, 0.01-0.04% of Al, 0.005-0.025% of Ti, 0.008% or less of N, 0.08-0.12% of Nb, 0.02% or less of P, 0.002% or less of S, 0.05-0.3% of Cr, 0.4-0.9% of Ni, 0.3-0.5% of Mo, 0.05-0.3% of Cu, 0.0005-0.006% of Ca, 0.001-0.04% of V, and the balance of Fe and inevitable impurities, wherein a number of deposits having an average diameter of 20 nm or less per unit area in a cross section of the steel material may be 6.5*109/mm2 or greater.

## Claims

### Claim 1

A steel material for a low yield ratio, high-strength steel having excellent low-temperature toughness, the steel material comprising, by wt %, 0.03 to 0.065% of C, 0.05 to 0.3% of Si, 1.7 to 2.2% of Mn, 0.01 to 0.04% of Al, 0.005 to 0.025% of Ti, 0.008% or less of N, 0.08 to 0.12% of Nb, 0.02% or less of P, 0.002% or less of S, 0.05 to 0.3% of Cr, 0.4 to 0.9% of Ni, 0.3 to 0.5% of Mo, 0.05 to 0.3% of Cu, 0.0005 to 0.006% of Ca, 0.001 to 0.04% of V, and a balance of Fe and inevitable impurities, wherein the number of precipitates having an average diameter of 20 nm or less per unit area in a cross section of the steel material is 6.5*109/mm2 or greater.

### Claim 2 (depends on 1)

The steel material of claim 1, wherein the precipitates include TiC, NbC and (Ti, Nb)C precipitates.

### Claim 3 (depends on 1)

The steel material of claim 1, wherein the steel material satisfies Equation 1 below:
0.17[{Ti−0.8*(48/14)N}/48+{Nb−0.8*(93/14)N}/93]/(C/12)≤0.25 [Equation 1]
wherein C, Ti, Nb and N refer to contents of C, Ti, Nb and N, respectively.

### Claim 4 (depends on 1)

The steel material of claim 1, wherein the steel material satisfies Equation 2 below:
2≤Cr+3*Mo+2*Ni≤2.7 [Equation 2]
wherein Cr, Mo and Ni refer to contents of Cr, Mo and Ni, respectively.

### Claim 5 (depends on 1)

The steel material of claim 1, wherein the steel material comprises acicular ferrite, bainitic ferrite, granular bainite, and martensite-austenite (MA) as a microstructure.

### Claim 6 (depends on 5)

The steel material of claim 5, wherein the acicular ferrite is included by 80 to 90%, the bainitic ferrite is included by 4 to 12%, the granular bainite is included by 6% or less, and the martensite-austenite (MA) is included by 5% or less, by an area fraction.

### Claim 7 (depends on 5)

The steel material of claim 5, wherein an average effective grain size of the acicular ferrite is 15 μm or less, an average effective grain size of the bainitic ferrite is 20 μm or less, an average effective grain size of the granular bainite is 20 μm or less, and an average effective grain size of the martensite-austenite is 3 μm or less.

### Claim 8 (depends on 1)

The steel material of claim 1, wherein the steel material satisfies Equation 3 below:
100*(P+10*S)≤2.4 [Equation 3]
wherein P and S refer to contents of P and S, respectively.

### Claim 9 (depends on 1)

The steel material of claim 1, wherein an yield strength of the steel material in a 30° inclined direction with reference to a rolling direction of the steel material is 540 MPa or greater, and a tensile strength of the steel material is 670 MPa or greater.

### Claim 10 (depends on 1)

The steel material of claim 1, wherein an yield ratio of the steel material is less than 85% and an elongation percentage of the steel material is 39% or greater.

### Claim 11 (depends on 1)

The steel material of claim 1, wherein the steel material has a Charpy impact energy of 190 J or greater at −60° C., and a lowest temperature satisfying drop weight tear test (DWTT) shear area of 85% or greater is −18° C. or lower.

### Claim 12 (depends on 1)

The steel material of claim 1, wherein a thickness of the steel material is 23 mm or greater.

### Claim 13

A method for manufacturing a steel material for a low yield ratio, high-strength steel having excellent low-temperature toughness, the method comprising:
reheating a slab including, by wt %, 0.03 to 0.065% of C, 0.05 to 0.3% of Si, 1.7 to 2.2% of Mn, 0.01 to 0.04% of Al, 0.005 to 0.025% of Ti, 0.008% or less of N, 0.08 to 0.12% of Nb, 0.02% or less of P, 0.002% or less of S, 0.05 to 0.3% of Cr, 0.4 to 0.9% of Ni, 0.3 to 0.5% of Mo, 0.05 to 0.3% of Cu, 0.0005 to 0.006% of Ca, 0.001 to 0.04% of V, and the balance of Fe and inevitable impurities, and satisfying Equation 1 below in a temperature range of 1080 to 1180° C.;
maintaining the reheated slab at a temperature of 1140° C. or higher for 45 minutes and extracting the slab;
primarily rolling the extracted slab at a rolling termination temperature of 980 to 1100° C.;
primarily cooling the primarily rolled steel material to a non-recrystallization region temperature range at a cooling rate of 20 to 60° C./s;
secondarily rolling the primarily cooled steel material primarily cooled at the non-recrystallization region temperature;
secondarily cooling the second rolled steel material at a cooling rate of 10 to 40° C./s; and
coiling the second cooled steel material in a temperature range of 420 to 540° C. to manufacture the same.
0.17[{Ti−0.8*(48/14)N}/48+{Nb−0.8*(93/14)N}/93]/(C/12)≤0.25 [Equation 1]
wherein C, Ti, Nb, and N refer to contents of C, Ti, Nb and N, respectively.

### Claim 14 (depends on 13)

The method of claim 13, wherein the slab satisfies Equation 2 below:
2≤Cr+3*Mo+2*Ni≤2.7 [Equation 2]
wherein Cr, Mo, and Ni refer to contents of Cr, Mo and Ni, respectively.

### Claim 15 (depends on 13)

The method of claim 13, wherein the slab satisfies Equation 3 below.
100*(P+10*S)≤2.4 [Equation 3]
wherein P and S refer to contents of P and S, respectively.

### Claim 16 (depends on 13)

The method of claim 13, wherein the non-recrystallization region temperature may be a temperature range of 910 to 970° C.

### Claim 17 (depends on 13)

The method of claim 13, wherein a reduction ratio of the second rolling is 75 to 85%.

### Claim 18 (depends on 13)

The method of claim 13, wherein a termination temperature of the second rolling is Ar3+70° C. to Ar3+110° C.