# US 2020/0368947 A1 · Molding Compositions and Articles Made Thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0368947 A1
- Document ID: US20200368947A1
- Status: Published application
- Kind: A1
- Application number: 16/869,769
- Filed: 2020-05-08
- Published: 2020-11-26
- Earliest claimed: 2019-05-20
- Assignees: Kraton Polymers LLC
- Applicants: Kraton Polymers LLC
- Inventors: Richard Companje
- Web page: https://patentgrep.com/patent/US20200368947A1

## CPC

- B29C 45/0001: {characterised by the choice of material}
- C08L 23/12: Polypropene
- C08L 23/14: Copolymers of propene (C08L23/16 takes precedence)
- C08L 53/025: {modified}
- B29K 2009/06: SB polymers, i.e. butadiene-styrene polymers
- B29K 2023/06: {PE, i.e. polyethylene}
- B29K 2023/12: {PP, i.e. polypropylene}
- B29K 2023/16: {EPM, i.e. ethylene-propylene copolymers; EPDM, i.e. ethylene-propylene-diene copolymers; EPT, i.e. ethylene-propylene terpolymers}
- B29K 2096/04: Block polymers
- B29K 2995/0017: Heat stable
- B29K 2995/0022: Bright, glossy or shiny surface
- B29L 2031/3008: {Instrument panels}
- B29L 2031/302: {Trim strips}
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29L: INDEXING SCHEME ASSOCIATED WITH SUBCLASS B29C, RELATING TO PARTICULAR ARTICLES

## Abstract

Injection molded articles having improved scratch resistance and reduced gloss change after heat and UV aging are disclosed. The article is formed from a molding composition having a melt flow index of 50-350 g/10 (230° C., 2.16 kg) as measured by ASTM D1238-04, the composition consisting essentially of: a) 15-80 wt. % of a hydrogenated styrenic block copolymer having a melt index of at least 12 grams/10 minutes according to ASTM D1238 at 230° C. and 2.16 kg weight; b) 10-60 wt. % of a polypropylene having a melt flow index greater than 300 g/10 min, measured under 230° C./2.16 kg according to ISO 1133-1; and c) 5-25 wt. % of a thermoplastic vulcanizate having a Shore A hardness from 60-90 (15 sec, 23° C.) as measured according to ISO 868. The article has a gloss increase after 10 days of aging at 120° C. of less than 100%, relative to an initial gloss, as determined by PSA D47 1850.

## Claims

### Claim 1

An injection molded article formed from a molding composition consisting essentially of:
a) 15-80 wt. % of a hydrogenated styrenic block copolymer having a general formula: S-E-S, (S-E1)n, (S-E1)nS, (S-E1)nX or mixtures thereof, n has a value of 2 to 6 and X is a coupling agent residue,
wherein prior to hydrogenation,
the S block is a polystyrene block having a molecular weight from 5,000 to 7,000,
the E block is a polydiene block, selected from the group consisting of polybutadiene, polyisoprene and mixtures thereof, having a molecular weight of from 30,000 to 70,000,
the E1 block is a polydiene block, selected from the group consisting of polybutadiene, polyisoprene and mixtures thereof, having a molecular weight of from 15,000 to 35,000;
b) 10-60 wt. % of a polypropylene; and
c) 5-25 wt. % of a thermoplastic vulcanizate;
wherein the hydrogenated styrenic block copolymer has a melt index of at least 12 g/10 minutes according to ASTM D1238 at 230° C. and 2.16 kg weight;
wherein the polypropylene has a melt flow index greater than 300g/10 min as measured according to ISO 1133-1 condition 230° C./2.16 kg;
wherein the thermoplastic vulcanizate has a Shore A hardness from 60-90 (15 sec, 23° C.) as measured according to ISO 868;
wherein the molding composition has a melt flow index of 50-350 g/10 (230° C., 2.16 kg) as measured by ASTM D1238-04; and
wherein the injection molded article, after 10 days of aging at 120° C., has a % gloss increase of less than 100, relative to an initial gloss, as determined by PSA D47 1850.

### Claim 2 (depends on 1)

The article of claim 1, wherein the thermoplastic vulcanizate is a dynamically vulcanized alloy consisting essentially of fully cured ethylene propylene diene methylene rubber particle encapsulated in a polypropylene matrix.

### Claim 3 (depends on 1)

The article of claim 1, wherein the thermoplastic vulcanizate has a density of from 0.880 to 0.980 g/cm3 as measured by ISO 1183.

### Claim 4 (depends on 1)

The article of claim 1, wherein the molding composition forms a layer having a thickness of at least 0.5 mm.

### Claim 5 (depends on 1)

The article of claim 1, wherein the polypropylene is selected from: (i) a homopolymer of propylene, (ii) a random copolymer of propylene and an olefin selected from ethylene and C4-C10 α-olefins, and (iii) a random terpolymer of propylene with two α-olefins selected from the group of ethylene and C4-C10 α-olefins.

### Claim 6 (depends on 1)

The article of claim 1, further comprising from 1-15 wt. % of one or more additives selected from the group consisting of a nucleating agent, a clarifier, a release agent, a plasticizer, an antioxidant, a thermal stabilizer, a visible light stabilizer, an ultraviolet light stabilizer, a colorant, a flame retardant, a lubricant, a synergist, a mold release agent, a flow enhancer, an anti-static agent, a filler, a scratch resistance additive, and a surface modifier.

### Claim 7 (depends on 1)

The article of claim 1, wherein the article is formed by any of injection molding, overmolding, rotomolding, thermoforming, casting, extrusion, profile extrusion, and blow molding.

### Claim 8 (depends on 1)

The article of claim 1, wherein the article is a vehicle interior product having positive scratch resistance, wherein the article is selected from interior trim, interior sheathing, door panels, instrument panels, and consoles.

### Claim 9 (depends on 1)

The article of claim 1, having a gloss at 60° C. of less than or equal to 10 as measured by PSA D47 1850.

### Claim 10 (depends on 1)

The article of claim 1, having a gloss after 10 days of aging at 120° C. of less than or equal to 15 as measured by PSA D47 1850.

### Claim 11

A method of preparing an injection molded article formed by:
(a) forming a molding composition, said molding composition consisting essentially of:
a) 15-80 wt. % of a hydrogenated styrenic block copolymer having a general formula: S-E-S, (S-E1)n, (S-E1)nS, (S-E1)nX or mixtures thereof, n has a value of 2 to 6 and X is a coupling agent residue,
wherein prior to hydrogenation,
the S block is a polystyrene block having a molecular weight from 5,000 to 7,000,
the E block is a polydiene block, selected from the group consisting of polybutadiene, polyisoprene and mixtures thereof, having a molecular weight of from 30,000 to 70,000,
the E1 block is a polydiene block, selected from the group consisting of polybutadiene, polyisoprene and mixtures thereof, having a molecular weight of from 15,000 to 35,000;
b) 10-55 wt. % of a polypropylene; and
c) 5-20 wt. % thermoplastic vulcanizate; and
(b) forming the injection molded article from the molding composition by injection molding, overmolding, rotomolding, thermoforming, casting, extrusion, profile extrusion, or blow molding;
wherein the injection molded article after 10 days of aging at 120° C. has a gloss that is at least 100% greater than the gloss of the article prior to the aging, as determined by PSA D47 1850.

### Claim 12 (depends on 11)

The method of claim 11, wherein the molding composition has a melt flow index of 50-350 g/10 (230° C., 2.16 kg) as measured by ASTM D1238-04.

### Claim 13 (depends on 11)

The method of claim 11, wherein step (b) comprises forming a layer having a thickness of at least 0.5 mm.

### Claim 14 (depends on 11)

The method of claim 11, wherein the article is a vehicle interior product having positive scratch resistance, wherein the article is selected from interior trim, interior sheathing, door panels, instrument panels, and consoles.

### Claim 15

An injection molded article formed from a molding composition consisting essentially of:
a) 40-80 wt. % of a hydrogenated styrenic block copolymer having a general formula: S-E-S, (S-E1)n, (S-E1)nS, (S-E1)nX or mixtures thereof, n has a value of 2 to 6 and X is a coupling agent residue,
wherein prior to hydrogenation,
the S block is a polystyrene block having a molecular weight from 5,000 to 7,000,
the E block is a polydiene block, selected from the group consisting of polybutadiene, polyisoprene and mixtures thereof, having a molecular weight of from 30,000 to 70,000,
the E1 block is a polydiene block, selected from the group consisting of polybutadiene, polyisoprene and mixtures thereof, having a molecular weight of from 15,000 to 35,000;
b) 15-40 wt. % of a polypropylene; and
c) 10-20 wt. % of a thermoplastic vulcanizate;
wherein the hydrogenated styrenic block copolymer has a melt index of at least 12 g/10 minutes according to ASTM D1238 at 230° C. and 2.16 kg weight;
wherein the polypropylene has a melt flow index greater than 300 g/10 min as measured according to ISO 1133-1 condition 230° C./2.16 kg;
wherein the thermoplastic vulcanizate has a Shore A hardness from 60-90 (15 sec, 23° C.) as measured according to ISO 868;
wherein the molding composition has a melt flow index of 50-250 g/10 (230° C., 2.16 kg) as measured by ASTM D1238-04; and
wherein the injection molded article, after 10 days of aging at 120° C., has a % gloss increase of less than 100, relative to an initial gloss, as determined by PSA D47 1850.

### Claim 16 (depends on 15)

The article of claim 15, wherein the thermoplastic vulcanizate is a dynamically vulcanized alloy consisting essentially of fully cured ethylene propylene diene methylene rubber particle encapsulated in a polypropylene matrix.

### Claim 17 (depends on 15)

The article of claim 15, wherein the polypropylene is selected from: (i) a homopolymer of propylene, (ii) a random copolymer of propylene and an olefin selected from ethylene and C4-C10 α-olefins, and (iii) a random terpolymer of propylene with two α-olefins selected from the group of ethylene and C4-C10 α-olefins.

### Claim 18 (depends on 15)

The article of claim 15, further comprising from 1-15 wt. % of one or more additives selected from the group consisting of a nucleating agent, a clarifier, a release agent, a plasticizer, an antioxidant, a thermal stabilizer, a visible light stabilizer, an ultraviolet light stabilizer, a colorant, a flame retardant, a lubricant, a synergist, a mold release agent, a flow enhancer, an anti-static agent, a filler, a scratch resistance additive, and a surface modifier.

### Claim 19 (depends on 15)

The article of claim 15, wherein the article is formed by any of injection molding, overmolding, rotomolding, thermoforming, casting, extrusion, profile extrusion, and blow molding.

### Claim 20 (depends on 15)

The article of claim 15, wherein the article is a vehicle interior product including interior trim, interior sheathing, door panels, instrument panels, and consoles, having good heat stability, scratch resistance, and improved gloss values after aging.