# US 2020/0368695 A1 · Base material for membrane filter and method for producing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0368695 A1
- Document ID: US20200368695A1
- Status: Published application
- Kind: A1
- Application number: 16/990,183
- Filed: 2020-08-11
- Published: 2020-11-26
- Earliest claimed: 2018-03-30
- Assignees: NGK Insulators, Ltd.
- Applicants: Ngk Insulators, Ltd.
- Inventors: Koji HIEDA
- Web page: https://patentgrep.com/patent/US20200368695A1

## CPC

- B01D 71/025: {Aluminium oxide}
- B01D 67/00411: {by sintering}
- B01D 67/0083: {Thermal after-treatment}
- B01D 69/02: characterised by their properties
- B01D 69/043: {characterised by the tube diameter}
- B01D 71/024: {Oxides}
- C04B 35/117: Composites
- C04B 38/0006: {Honeycomb structures (from one or more corrugated sheets by winding or stacking C04B38/0083)}
- B01D 2323/08: Specific temperatures applied
- B01D 2325/0283: Pore size
- B01D 2325/02833: more than 10 and up to 100 nm
- B01D 2325/20: Specific permeability or cut-off range
- B01D 2325/24: Mechanical properties, e.g. strength
- C04B 2111/00129: {Extrudable mixtures}
- C04B 2111/00612: {as one or more layers of a layered structure}
- C04B 2111/00793: {as filters or diaphragms}
- C04B 2235/3217: Aluminum oxide or oxide forming salts thereof, e.g. bauxite, alpha-alumina
- C04B 2235/3232: Titanium oxides or titanates, e.g. rutile or anatase
- C04B 2235/5436: micrometer sized, i.e. from 1 to 100 micron
- C04B 2235/5445: submicron sized, i.e. from 0,1 to 1 micron
- C04B 2235/5454: nanometer sized, i.e. below 100 nm
- C04B 2235/6021: Extrusion moulding
- C04B 2235/6567: Treatment time
- C04B 2235/6583: Oxygen containing atmosphere, e.g. with changing oxygen pressures
- C04B 2235/72: Products characterised by the absence or the low content of specific components, e.g. alkali metal free alumina ceramics
- C04B 2235/96: Properties of ceramic products, e.g. mechanical properties such as strength, toughness, wear resistance
- B01D: SEPARATION (separating solids from solids by wet methods B03B, B03D; by pneumatic jigs or tables B03B; by other dry methods B07; magnetic or electrostatic separation of solid materials from solid materials or fluids, separation by high-voltage electric fields B03C; centrifuges, vortex apparatus B04; presses per se for squeezing-out liquid from liquid-containing material B30B9/02; treatment of water C02F, e.g. softening by ion-exchange C02F1/42; {arrangements of air intake cleaners in gas turbine plants F02C7/05} ; arrangements or mounting of filters in air-conditioning, air-humidification or ventilation F24F13/28)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE

## Abstract

A base material for a membrane filter contains 90% by mass or more of aluminum oxide and 0.1% by mass or more and 10% by mass or less of titanium oxide. In a pore distribution curve measured by a mercury porosimeter, the base material has a first peak and a second peak which is higher than the first peak and is located at a pore size larger than that of the first peak, and the volume of pores with a pore size of 7 μm or more is 0.02 cm3/g or more.

## Claims

### Claim 1

A base material for a membrane filter comprising 90% by mass or more of aluminum oxide and 0.1% by mass or more and 10% by mass or less of titanium oxide,
wherein, in a pore distribution curve measured by a mercury porosimeter, the base material has a first peak and a second peak which is higher than the first peak and is located at a pore size larger than that of the first peak, and the volume of pores with a pore size of 7 μm or more is 0.02 cm3/g or more.

### Claim 2 (depends on 1)

The base material for a membrane filter according to claim 1, wherein the first peak is located at a pore size in a range of 4 μm to 6 μm, and the second peak is located at a pore size in a range of 6 μm to 9 μm.

### Claim 3 (depends on 1)

The base material for a membrane filter according to claim 1, wherein, in the pore distribution curve measured by the mercury porosimeter, the volume of pores of the first peak is in a range of 0.005 cm3/g to 0.02 cm3/g, and the volume of pores of the second peak is in a range of 0.03 cm3/g to 0.05 cm3/g.

### Claim 4 (depends on 1)

The base material for a membrane filter according to claim 1, wherein the base material has a permeation rate of 7.5 m3/(m2·h) or more.

### Claim 5 (depends on 1)

The base material for a membrane filter according to claim 1, wherein the base material has an internal pressure strength of 0.6 MPa or more.

### Claim 6

A method for producing a base material for a membrane filter comprising:
a mixing and forming step in which, using, as raw materials, aluminum oxide having an average particle size of 35 μm or more and 45 μm or less and a purity of 90% by mass or more and titanium oxide having an average particle size of 0.01 μm or more and 1 μm or less and a purity of 70% by mass or more, mixing is performed such that the amount of aluminum oxide is 90% by mass or more and the amount of titanium oxide is 0.1% by mass or more and 10% by mass or less based on the total of aluminum oxide and titanium oxide, and the resulting mixture is formed into a shaped body; and
a firing step in which the shaped body is fired in an oxidizing atmosphere in a temperature range of 1,400° C. to 1,600° C.

### Claim 7 (depends on 6)

The method for producing a base material for a membrane filter according to claim 6, wherein, in the mixing and forming step, the average particle size of the aluminum oxide is adjusted to 35 μm or more and 45 μm or less by mixing aluminum oxide powders with an average particle size of 0.5 μm or more and 50 μm or less.

### Claim 8 (depends on 6)

The method for producing a base material for a membrane filter according to claim 6, wherein, in the mixing and forming step, one or more raw materials selected from the group consisting of (1) to (5) are used:
(1) aluminum oxide having an average particle size of 37 μm or more and 43 μm or less,
(2) aluminum oxide having a purity of 95% by mass or more and 99.9% by mass or less,
(3) titanium oxide having a purity of 85% by mass or more and 99.9% by mass or less,
(4) titanium oxide mixed in an amount of 0.1% by mass or more and 2% by mass or less, and
(5) aluminum oxide in an amount of 98% by mass or more and 99.9% by mass or less.

### Claim 9 (depends on 6)

The method for producing a base material for a membrane filter according to claim 6, wherein, in the mixing and forming step, the mixture is formed into one or more shapes selected from the group consisting of (6) to (8):
(6) a shape with a diameter of 30 mm or more, a length of 100 mm or more, and 19 or more cells,
(7) a shape with a diameter of 90 mm or more, a length of 100 mm or more, and 300 or more cells, and
(8) a shape with a diameter of 180 mm or more, a length of 500 mm or more, and 2,000 or more cells.