# US 2020/0347489 A1 · Al plated welded pipe for hardening use and al plated hollow member and method for producing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0347489 A1
- Document ID: US20200347489A1
- Status: Published application
- Kind: A1
- Application number: 16/753,961
- Filed: 2017-11-20
- Published: 2020-11-05
- Earliest claimed: 2017-11-20
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Jun MAKI; Soshi FUJITA; Toyomitsu NAKAMURA
- Web page: https://patentgrep.com/patent/US20200347489A1

## CPC

- C22C 38/54: with boron
- B23K 11/002: {specially adapted for particular articles or work}
- B23K 11/0873: {of the longitudinal seam of tubes}
- B23K 11/163: {Welding of coated materials}
- B23K 35/0261: {Rods, electrodes or wires}
- B23K 35/3053: {Fe as the principal constituent}
- C21D 9/08: for tubular bodies or pipes
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/12: Aluminium or alloys based thereon
- C23C 2/26: After-treatment (C23C2/14 takes precedence)
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/29: {Cooling or quenching}
- C23C 2/38: Wires; Tubes
- C23C 2/40: Plates; Strips
- C23C 28/00: Coating for obtaining at least two superposed coatings either by methods not provided for in a single one of groups C23C2/00 - C23C26/00 or by combinations of methods provided for in subclasses C23C and C25C or C25D
- C25D 3/44: Aluminium
- C25D 7/04: Tubes; Rings; Hollow bodies
- B23K 13/046: {for tubes}
- B23K 2101/06: Tubes
- B23K 2103/04: Steel {or steel} alloys
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

An Al plated electric resistance welded steel pipe for hardening use suppressing the formation of scale to the inside of the plating layer while performing hot forming and an Al plated hollow member using that Al plated electric resistance welded steel pipe, wherein the Al plated electric resistance welded steel pipe for hardening use is comprised of a base material made of a tubular steel plate and having a predetermined chemical composition and an electric resistance welded zone provided at a seam portion of the steel plate and extending in a longitudinal direction of the steel plate, the base material is further provided with an intermetallic compound layer positioned on the surface of the steel plate and including an Al-Fe-Si-based intermetallic compound and an Al plating layer positioned on the surface of the intermetallic compound layer and containing Al and Si, and 70×X/D≤Y/t≤30 is satisfied, wherein X (μm) is a thickness of the intermetallic compound layer, Y (μm) is a thickness of the Al plating layer, t (mm) is a pipe thickness of the steel pipe, and D (mm) is an outside diameter of the steel pipe.

## Claims

### Claim 1

An Al plated electric resistance welded steel pipe for hardening use comprising a base material made of a tubular steel plate and an electric resistance welded zone provided at a seam portion of the steel plate and extending in a longitudinal direction of the steel plate,
the base material comprising, by mass %,
C: 0.06 to 0.50%,
Si: 0.01 to 0.80%,
Mn: 0.60 to 3.00%,
P: 0.050% or less,
S: 0.050% or less,
Al: 0.10% or less,
O: 0.006% or less,
N: 0.020% or less,
Ti: 0.01 to 0.10%,
B: 0 to 0.1000%,
Nb: 0 to 0.10%,
V: 0 to 0.30%,
Cr: 0 to 0.50%,
Mo: 0 to 0.50%,
Ni: 0 to 0.50%,
Cu: 0 to 0.50%,
Ca: 0. to 0.005%,
REM: 0 to 0.005% and
a balance of Fe and impurities,
the base material comprising
an intermetallic compound layer positioned on the surface of the steel plate and including an Al-Fe-Si-based intermetallic compound and
an Al plating layer positioned on the surface of the intermetallic compound layer and containing Al and Si,
wherein
70×X/D≤Y/t≤30
is satisfied, wherein X (μm) is a thickness of the intermetallic compound layer, Y (μm) is a thickness of the Al plating layer, t (mm) is a pipe thickness of the steel pipe, and D (mm) is an outside diameter of the steel pipe.

### Claim 2 (depends on 1)

The Al plated electric resistance welded steel pipe for hardening use according to claim 1, wherein X≤5.0, Y≤32, and 4.0≤Y/X≤6.0 are satisfied.

### Claim 3 (depends on 1)

The Al plated electric resistance welded steel pipe for hardening use according to claim 1, wherein the surface of the Al plating layer is further provided with a film mainly comprised of ZnO and the amount of deposition of the film is, by amount of Zn, 0.1 to 1 g/m2.

### Claim 4 (depends on 1)

The Al plated electric resistance welded steel pipe for hardening use according to claim 1 wherein the welded zone is covered by an alloy mainly comprised of Al.

### Claim 5 (depends on 1)

The Al plated electric resistance welded steel pipe for hardening use according to claim 1 wherein 2%≤t/D≤10% is satisfied.

### Claim 6

An Al plated hollow member comprising:
an electric resistance welded pipe comprising a base material made of a tubular steel plate and an electric resistance welded zone provided at a seam portion of the steel plate and extending in a longitudinal direction of the steel plate, the base material comprising, by mass %,
C: 0.06 to 0.50%,
Si: 0.01 to 0.80%,
Mn: 0.60 to 3.00%,
P: 0.050% or less,
S: 0.050% or less,
Al: 0.10% or less,
O: 0.006% or less,
N: 0.020% or less,
Ti: 0.01 to 0.10%,
B: 0 to 0.1000%,
Nb: 0 to 0.10%,
V: 0 to 0.30%,
Cr: 0 to 0.50%,
Mo: 0 to 0.50%,
Ni: 0 to 0.50%,
Cu: 0 to 0.50%,
Ca: 0. to 0.005%,
REM: 0 to 0.005% and
a balance of Fe and impurities; and
an alloy layer positioned on the surface of the electric resistance welded steel pipe and containing at least one of an Al-Fe-based alloy and Al-Fe-Si-based alloy,
wherein
a rate of formation of Fe oxide scale in the alloy layer is 5% or less, and
a Vickers hardness Hv of a steel base material of the electric resistance welded pipe is 350 to 800.

### Claim 7 (depends on 6)

The Al plated hollow member according to claim 6, wherein there is no Al not alloyed remaining in the alloy layer.

### Claim 8 (depends on 6)

The Al plated hollow member according to claim 6, wherein
the surface of the alloy layer is further provided with a film mainly comprised of ZnO, and
the amount of deposition of the film is, by amount of Zn, 0.1 to 1 g/m2.

### Claim 9

A method for producing an Al plated hollow member comprising:
a heating step of heating by a heating temperature of 850° C. or more an Al plated electric resistance welded steel pipe for hardening use comprising a base material made of a tubular steel plate and an electric resistance welded zone provided at a seam portion of the steel plate and extending in a longitudinal direction of the steel plate, wherein
the base material contains, by mass %,
C: 0.06 to 0.50%,
Si: 0.01 to 0.80%,
Mn: 0.60 to 3.00%,
P: 0.050% or less,
S: 0.050% or less,
Al: 0.10% or less,
O: 0.006% or less,
N: 0.020% or less,
Ti: 0.01 to 0.10%,
B: 0 to 0.1000%,
Nb: 0 to 0.10%,
V: 0 to 0.30%,
Cr: 0 to 0.50%,
Mo: 0 to 0.50%,
Ni: 0 to 0.50%,
Cu: 0 to 0.50%,
Ca: 0. to 0.005%,
REM: 0 to 0.005% and
a balance of Fe and impurities, and
the base material is further provided with
an intermetallic compound layer positioned on the surface of the steel plate and including an Al-Fe-Si-based intermetallic compound and
an Al plating layer positioned on the surface of the intermetallic compound layer and containing Al and Si;
a forming step of forming the heated Al plated electric resistance welded steel pipe for hardening use into a desired shape; and
a rapid cooling step of rapid cooling the Al plated electric resistance welded steel pipe for hardening use formed into the desired shape by an average cooling rate of 20° C./s or more, wherein
the following formula (1) and formula (2) are satisfied, wherein X (μm) is a thickness of the intermetallic compound layer, Y (μm) is a thickness of the Al plating layer, t (mm) is a pipe thickness of the steel pipe, D (mm) is an outside diameter of the steel pipe, and HR (° C./s) is an average rate of temperature rise from ordinary temperature to a peak temperature −50° C. set at the time of hot forming:
Y/X≥α×t/D (1)
α=168×HR−0.45 (2).

### Claim 10 (depends on 2)

The Al plated electric resistance welded steel pipe for hardening use according to claim 2, wherein the surface of the Al plating layer is further provided with a film mainly comprised of ZnO and the amount of deposition of the film is, by amount of Zn, 0.1 to 1 g/m2.

### Claim 11 (depends on 2)

The Al plated electric resistance welded steel pipe for hardening use according to claim 2 wherein the welded zone is covered by an alloy mainly comprised of Al.

### Claim 12 (depends on 2)

The Al plated electric resistance welded steel pipe for hardening use according to claim 2 wherein 2%≤t/D≤10% is satisfied.

### Claim 13 (depends on 3)

The Al plated electric resistance welded steel pipe for hardening use according to claim 3 wherein the welded zone is covered by an alloy mainly comprised of Al.

### Claim 14 (depends on 3)

The Al plated electric resistance welded steel pipe for hardening use according to claim 3 wherein 2%≤t/D≤10% is satisfied.

### Claim 15 (depends on 4)

The Al plated electric resistance welded steel pipe for hardening use according to claim 4 wherein 2%≤t/D≤10% is satisfied.

### Claim 16 (depends on 7)

The Al plated hollow member according to claim 7, wherein
the surface of the alloy layer is further provided with a film mainly comprised of ZnO, and
the amount of deposition of the film is, by amount of Zn, 0.1 to 1 g/m2.