# US 2020/0347476 A1 · High-strength steel sheet having excellent processability and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0347476 A1
- Document ID: US20200347476A1
- Status: Published application
- Kind: A1
- Application number: 16/767,858
- Filed: 2018-10-11
- Published: 2020-11-05
- Earliest claimed: 2017-12-22
- Assignees: Posco
- Applicants: Posco
- Inventors: Yeon-Sang AHN; Chang-Hyo SEO; Kang-Hyun CHOI; Eul-Yong CHOI
- Web page: https://patentgrep.com/patent/US20200347476A1

## CPC

- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 9/46: for sheet metals
- C21D 1/26: Methods of annealing
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/04: to produce plates or strips for drawing, e.g. for deep-drawing
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/32: with boron
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/29: {Cooling or quenching}
- C23C 2/40: Plates; Strips
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C22C 38/22: with molybdenum or tungsten
- C22C 38/38: with more than 1.5% by weight of manganese
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

Provided is a high-strength steel sheet having a tensile strength of 780 MPa or higher. The high-strength steel sheet has a low yield ratio and excellent ductility (El) and strain hardening exponent (n) and thus has enhanced processability.

## Claims

### Claim 1

A high strength steel sheet having excellent workability, comprising:
in weight %, 0.06 to 0.18% of carbon (C), 1.5% or less (excluding 0%) of silicon (Si), 1.7 to 2.5% of manganese (Mn), 0.15% or less (excluding 0%) of molybdenum (Mo), 1.0% or less (excluding 0%) of chromium (Cr), 0.1% or less of phosphorus (P), 0.01% or less of sulfur (S), 1.0% or less (excluding 0%) of aluminum (Al), 0.001 to 0.04% of titanium (Ti), 0.001 to 0.04% of niobium (Nb), 0.01% or less of nitrogen (N), 0.01% or less (excluding 0%) of boron (B), 0.05% or less (excluding 0%) of antimony (Sb), and a remainder of Fe and other inevitable impurities, and
as a microstructure, ferrite having an area fraction of 40% or more and bainite, fresh martensite, and retained austenite as a remainder,
wherein a ratio (Mb/Mt) of a total fraction (Mt) of the fresh martensite and a fraction (Mb) of fresh martensite adjacent to the bainite is 60% or more, and a ratio (Ms/Mt) of the total fraction (Mt) of the fresh martensite and a fraction (Ms) of fine fresh martensite having an average particle size of 3 μm or less is 60% or more.

### Claim 2 (depends on 1)

The high strength steel sheet having excellent workability of claim 1, wherein in the high strength steel sheet, a relationship of C, Si, Al, Mn, Mo and Cr satisfies the following relationship 1,
(Si+Al+C)/(Mn+Mo+Cr)≥0.25 [Relationship 1]
where respective elements indicate a weight content.

### Claim 3 (depends on 1)

The high strength steel sheet having excellent workability of claim 1, wherein the high strength steel sheet comprises a zinc-based plating layer on at least one surface.

### Claim 4 (depends on 1)

The high strength steel sheet having excellent workability of claim 1, wherein the high strength steel sheet has a tensile strength of 780 MPa or more, and a relationship between a strain hardening coefficient (n), a ductility (El), a tensile strength (TS), and a yield ratio (YR) measured in a strain section of 4 to 6% satisfies the following relationship 2,
(n×El×TS)/YR≥5000[Relationship 2]
where the unit is MPa %.

### Claim 5

A method of manufacturing a high strength steel sheet having excellent workability, the method comprising:
reheating, at a temperature in a range of 1050 to 1300° C., a steel slab including, in weight %, 0.06 to 0.18% of carbon (C), 1.5% or less (excluding 0%) of silicon (Si), 1.7 to 2.5% of manganese (Mn), 0.15% or less (excluding 0%) of molybdenum (Mo), 1.0% or less (excluding 0%) of chromium (Cr), 0.1% or less of phosphorus (P), 0.01% or less of sulfur (S), 1.0% or less (excluding 0%) of aluminum (Al), 0.001 to 0.04% of titanium (Ti), 0.001 to 0.04% of niobium (Nb), 0.01% or less of nitrogen (N), 0.01% or less (excluding 0%) of boron (B), 0.05% or less (excluding 0%) of antimony (Sb), a remainder of Fe and other inevitable impurities;
preparing a hot-rolled steel sheet by finishing hot-rolling the reheated steel slab at an Ar3 transformation point or higher;
coiling the hot rolled steel sheet in a temperature range of 400 to 700° C.;
after the coiling, primary cooling at a cooling rate of 0.1° C./s or less to room temperature;
after the cooling, producing a cold rolled steel sheet by cold rolling at a cold reduction ratio of 40 to 70%;
continuously annealing the cold rolled steel sheet in a temperature range of Ac1+30° C. to Ac3−20° C.;
after the continuously annealing, performing a secondary cooling at a cooling rate of 10° C./s or less (excluding 0° C./s) to 630 to 670° C.;
after the secondary cooling, performing a third cooling to 400 to 500° C. at a cooling rate of 5° C./s or more in a hydrogen cooling facility;
maintaining for 70 seconds or more after the third cooling;
hot-dip galvanizing after the maintaining; and
after the hot-dip galvanizing, performing a final cooling to Ms or less at a cooling rate of 1° C./s or more.

### Claim 6 (depends on 5)

The method of manufacturing a high-strength steel sheet having excellent workability of claim 5, wherein in the steel slab, a relationship of C, Si, Al, Mn, Mo and Cr satisfies the following relation 1,
(Si+Al+C)/(Mn+Mo+Cr)≥0.25 [Relationship 1]
where respective elements indicate a weight content.

### Claim 7 (depends on 5)

The method of manufacturing a high-strength steel sheet having excellent workability of claim 5, wherein a temperature at an outlet side during the finishing hot-rolling satisfies Ar3 to Ar3+50° C.

### Claim 8 (depends on 5)

The method of manufacturing a high-strength steel sheet having excellent workability of claim 5, wherein a bainite phase is formed upon the third cooling.

### Claim 9 (depends on 5)

The method of manufacturing a high-strength steel sheet having excellent workability of claim 5, wherein a fresh martensite phase is formed upon the final cooling after the hot-dip galvanizing.

### Claim 10 (depends on 5)

The method of manufacturing a high-strength steel sheet having excellent workability of claim 5, wherein the hot-dip galvanizing is performed in a zinc plating bath at 430 to 490° C.

### Claim 11 (depends on 5)

The method of manufacturing a high-strength steel sheet having excellent workability of claim 5, further comprising temper rolling at a reduction ratio of less than 1.0% after the final cooling.