# US 2020/0270713 A1 · Method for producing a high strength coated steel sheet having improved ductility and formability, and obtained coated steel sheet

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0270713 A1
- Document ID: US20200270713A1
- Status: Published application
- Kind: A1
- Application number: 16/063,740
- Filed: 2016-12-21
- Published: 2020-08-27
- Earliest claimed: 2015-12-21
- Assignees: ArcelorMittal
- Applicants: ArcelorMittal
- Inventors: Maya GOSPODINOVA; Véronique HEBERT
- Web page: https://patentgrep.com/patent/US20200270713A1

## CPC

- C21D 8/0236: {Cold rolling}
- C21D 9/46: for sheet metals
- B23K 11/11: Spot welding
- B23K 35/3073: {with Mn as next major constituent}
- C21D 1/19: by interrupted quenching
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0247: characterised by the heat treatment
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/26: with niobium or tantalum
- C22C 38/34: with more than 1.5% by weight of silicon
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/29: {Cooling or quenching}
- C23C 2/40: Plates; Strips
- B23K 2103/04: Steel {or steel} alloys
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A method for producing a coated steel sheet having a tensile strength TS of at least 1100 MPa, a total elongation TE according to ISO standard 6892-1 of at least 12%, the product TSxTE of the tensile strength by the total elongation being at least 14200 MPa %, and a hole expansion ratio HER according to ISO standard 16630:2009 of at least 25%, the method including the following successive steps: providing a cold-rolled steel sheet, the chemical composition of the steel containing in weight %: 0.15%≤C≤0.23%, 2.0%≤Mn≤2.7%, with C+Mn/10≥0.420%, 0≤Cr≤0.40%, with Mn+Cr≥2.25%, 0.2%≤Si≤1.6%, 0.02%≤Al≤1.2%, with 1.0%≤Si+Al≤2.2%, 0≤Nb≤0.035%, 0≤Mo≤0.1%, the remainder being Fe and unavoidable impurities, annealing the steel sheet at an annealing temperature TA so as to obtain a structure comprising at least 65% of austenite and at most 35% of intercritical ferrite, quenching the sheet from a temperature of at least 600° C. at a cooling rate comprised between 20° C./s and 50° C./s down to a quenching temperature QT between 200° C. and 270° C., heating the sheet up to a partitioning temperature PT comprised between 400° C. and 480° C. and maintaining the sheet at this partitioning temperature PT for a partitioning time Pt comprised between 50 s and 250 s, hot-dip coating the sheet at a temperature less than 515° C., cooling the coated sheet down to the room temperature, the steel sheet having a microstructure consisting of, in surface fraction: between 3% and 15% of retained austenite, at least 30% of tempered martensite, at most 5% of fresh martensite, at most 35% of bainite, the sum of the surface fractions of tempered martensite, fresh martensite and bainite being comprised between 55% and 92%, and between 5% and 35% of ferrite.

## Claims

### Claim at position 1

1-31. (canceled)

### Claim 32

A method for producing a coated steel sheet having a tensile strength TS of at least 1100 MPa, a total elongation TE according to ISO standard 6892-1 of at least 12%, a product TSxTE of the tensile strength by the total elongation of at least 14200 MPa %, and a hole expansion ratio HER according to ISO standard 16630:2009 of at least 25%, wherein the method comprises the following successive steps:
providing a cold-rolled steel sheet made of a steel having a chemical composition containing by weight:
0.15%≤C≤0.23%,
2.0%≤Mn≤2.7%,
with C+Mn/10≥0.420%,
0≤Cr≤0.40%,
with Mn+Cr≥2.25%,
0.2%≤Si≤1.6%,
0.02%≤Al≤1.2%,
with 1.0%≤Si+Al≤2.2%,
0≤Nb≤0.035%,
0≤Mo≤0.1%, and
a remainder, the remainder being Fe and unavoidable impurities,
annealing the steel sheet at an annealing temperature TA so as to obtain a structure comprising at least 65% of austenite and at most 35% of intercritical ferrite,
quenching the steel sheet from a temperature of at least 600° C. at a cooling rate comprised between 20° C./s and 50° C./s down to a quenching temperature QT between 200° C. and 270° C.,
heating the steel sheet up to a partitioning temperature PT comprised between 400° C. and 480° C. and maintaining the steel sheet at the partitioning temperature PT for a partitioning time Pt comprised between 50 s and 250 s,
hot-dip coating the steel sheet at a temperature less than 515° C.,
cooling the coated steel sheet down to the room temperature,
the coated steel sheet having a microstructure consisting of, in surface fraction:
between 3% and 15% of retained austenite,
at least 30% of tempered martensite,
at most 5% of fresh martensite,
at most 35% of bainite,
a sum of the surface fractions of tempered martensite, fresh martensite and bainite being comprised between 55% and 92%,
between 5% and 35% of ferrite.

### Claim 33 (depends on 32)

The method according to claim 32, wherein the method comprises, between the annealing step and the quenching step, a step of slow cooling the steel sheet at a cooling rate lower than 10° C./s for a time of at least 10 s down to the temperature of at least 600° C.

### Claim 34 (depends on 33)

The method according to claim 33, wherein the ferrite comprises, in area fraction with respect to the whole structure, between 0% and 5% of intercritical ferrite and between 0% and 35% of transformation ferrite, the transformation ferrite being formed during the slow cooling step.

### Claim 35 (depends on 32)

The method according to claim 32, wherein the ferrite consists of intercritical ferrite.

### Claim 36 (depends on 32)

The method according to claim 32, wherein the steel sheet has, just before the heating to the partitioning temperature PT, a structure consisting of between 5% and 35% of ferrite, at least 3% of austenite, at least 30% of martensite, and a complement consisting of lower bainite.

### Claim 37 (depends on 32)

The method according to claim 32, wherein the step of providing the cold-rolled steel sheet comprises:
hot rolling a sheet made of said steel to obtain a hot rolled steel sheet,
coiling said hot-rolled steel sheet at a temperature Tc comprises between 400° C. and 650° C., to obtain a hot-rolled and coiled steel sheet,
performing a heat treatment at a temperature THBA comprised between 400° C. and 700° C., the hot-rolled and coiled steel sheet being maintained at said temperature THBA for a time between 120 s and 15 hours,
cold rolling said hot-rolled steel sheet to obtain said cold-rolled steel sheet.

### Claim 38 (depends on 37)

The method according to claim 37, wherein the heat treatment is a batch annealing performed on the hot-rolled and coiled steel sheet, the temperature THBA being comprised between 550° C. and 700° C., the hot-rolled and coiled sheet being maintained at said temperature THBA for a time between 5 and 15 hours.

### Claim 39 (depends on 37)

The method according to claim 37, wherein the heat treatment is a continuous annealing, the temperature THBA being comprised between 600° C. and 700° C., the hot-rolled and coiled steel sheet being maintained at said temperature THBA for a time between 120 s and 360 s.

### Claim 40 (depends on 32)

The method according to claim 32, wherein, after the steel sheet is quenched to the quenching temperature QT and before the steel sheet is heated to the partitioning temperature PT, the steel sheet is held at the quenching temperature QT for a holding time comprised between 2 s and 8 s.

### Claim 41 (depends on 32)

The method according to claim 32, wherein the chemical composition of the steel satisfies at least one of the following conditions:
C≥0.17%,
C≤0.21%,
Mn≤2.5%,
0.010%≤Nb,
Cr≤0.05%, or
Cr≥0.10%.

### Claim 42 (depends on 41)

The method according to claim 41, wherein the chemical composition of the steel is such that C+Si/10≤0.30% and Al≥6(C+Mn/10)−2.5%.

### Claim 43 (depends on 41)

The method according to claim 41, wherein the chemical composition of the steel is such that 0.2%≤Si<1.0% and 0.4%≤Al≤1.2%.

### Claim 44 (depends on 43)

The method according to claim 43, wherein 0.2%≤Si≤0.8% and 0.7%≤Al≤1.2%.

### Claim 45 (depends on 32)

The method according to claim 32, wherein the hot-dip coating step is a galvanizing step, or a galvannealing step with an alloying temperature GAT comprised between 480° C. and 515° C.

### Claim 46 (depends on 32)

The method according to claim 32, wherein the steel sheet is coated with Zn or a Zn alloy.

### Claim 47 (depends on 41)

A process for producing a resistance spot weld of at least two steel sheets, said process comprising:
producing a first coated steel sheet by a method according to claim 41, the first coated steel sheet being coated with Zn or a Zn alloy,
providing a second steel sheet made of a steel having a composition such that C+Si/10≤0.30% and Al≥6(C+Mn/10)−2.5%,
resistance spot welding said first coated steel sheet to said second steel sheet.

### Claim 48

A coated steel sheet, wherein the coated steel sheet is made of a steel having a chemical composition containing by weight:
0.15%≤C≤0.23%,
2.0%≤Mn≤2.7%,
with C+Mn/10≥0.420%,
0≤Cr≤0.40%,
with Mn+Cr≥2.25%,
0.2%≤Si≤1.6%,
0.02%≤Al≤1.2%,
with 1.0%≤Si+Al≤2.2%,
0≤Nb≤0.035%,
0≤Mo≤0.1%,
and a remainder, the remainder being Fe and unavoidable impurities,
said coated steel sheet having a microstructure consisting of, in surface percentage:
between 3% and 15% of retained austenite,
at least 30% of tempered martensite,
at most 5% of fresh martensite,
at most 35% of bainite,
a sum of the surface fractions of tempered martensite, fresh martensite and bainite being comprised between 55% and 92%,
between 5% and 35% of ferrite.

### Claim 49 (depends on 48)

The coated steel sheet according to claim 48, wherein the ferrite comprises, in area fraction with respect to the whole structure, between 0% and 5% of intercritical ferrite and between 0% and 35% of transformation ferrite.

### Claim 50 (depends on 48)

The coated steel sheet according to claim 48, wherein the ferrite consists of intercritical ferrite.

### Claim 51 (depends on 48)

The coated steel sheet according to claim 48, wherein the retained austenite has a C content comprised between 0.9% and 1.2%.

### Claim 52 (depends on 48)

The coated steel sheet according to claim 48, wherein the coated steel sheet has a yield strength of at least 500 MPa, a tensile strength of at least 1100 MPa, a total elongation according to ISO 6892-1 of at least 12%, a product TSxTE of the tensile strength by the total elongation of at least 14200 MPa %, and a hole expansion ratio HER according to ISO 16630:2009 of at least 25%.

### Claim 53 (depends on 48)

The coated steel sheet according to claim 48, wherein the chemical composition of the steel satisfies at least one of the following conditions:
C≥0.17%,
C≤0.21%,
Mn≤2.5%,
0.010%≤Nb,
Cr≤0.05%, or
Cr≥0.10%.

### Claim 54 (depends on 48)

The coated steel sheet according to claim 48, wherein the chemical composition of the steel is such that C+Si/10≤0.30% and Al≥6(C+Mn/10)−2.5%.

### Claim 55 (depends on 54)

The coated steel sheet according to claim 54, wherein the chemical composition of the steel is such that 0.2%≤Si<1.0% and 0.4%≤Al≤1.2%.

### Claim 56 (depends on 55)

The coated steel sheet according to claim 55, wherein 0.2%≤Si≤0.8% and 0.7%≤Al≤1.2%.

### Claim 57 (depends on 54)

The coated steel sheet according to claim 54, wherein the steel sheet is coated with Zn or a Zn alloy.

### Claim 58 (depends on 48)

The coated steel sheet according to claim 48, wherein the coated steel sheet has a thickness comprised between 0.7 and 3 mm.

### Claim 59 (depends on 57)

A welded structure comprising at least ten resistance spot welds of at least two steel sheets, wherein a first of said two steel sheets is the coated steel sheet according to claim 57, and a second of said two steel sheets is made of a steel having a composition such that C+Si/10≤0.30% and Al≥6(C+Mn/10)−2.5%, and wherein the at least ten resistance spot welds have a mean number of cracks per resistance spot weld of less than 6.

### Claim 60 (depends on 26, 59)

The welded structure according to claim 59, wherein the second steel sheet is according to claim 26.

### Claim 61 (depends on 32, 48)

A structural part of a motor vehicle comprising the coated steel sheet manufactured according to the method of claim 32, or the coated steel sheet according to claim 48.

### Claim 62 (depends on 47, 59)

A structural part of a motor vehicle comprising the resistance spot weld produced by the process according to claim 47, or of the welded structure according to claim 59.