# US 2020/0270165 A1 · Optical fiber and manufacuturing method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0270165 A1
- Document ID: US20200270165A1
- Status: Published application
- Kind: A1
- Application number: 16/322,122
- Filed: 2017-08-23
- Published: 2020-08-27
- Earliest claimed: 2017-08-23
- Assignees: Chengdu Futong Optical Communication Technologies Co., Ltd.
- Applicants: Chengdu Futong Optical Communication Technologies Co., Ltd.
- Inventors: Haibin CHEN; Jian CHEN; Qiang CHEN; Qingguo LI; Xiaosong JIAN
- Web page: https://patentgrep.com/patent/US20200270165A1

## CPC

- C03B 37/0142: {Reactant deposition burners}
- C03B 37/01473: {Collapsing}
- C03B 37/01446: {Thermal after-treatment of preforms, e.g. dehydrating, consolidating, sintering (C03B37/01853 takes precedence)}
- C03B 37/01493: {Deposition substrates, e.g. targets, mandrels, start rods or tubes}
- C03B 37/027: Fibres composed of different sorts of glass, {e.g. glass optical fibres}(C03B37/0253, C03B37/028 take precedence)
- G02B 6/02: Optical fibres with cladding {with or without a coating}
- C03B 2201/12: doped with fluorine (C03B2201/14 takes precedence)
- C03B 2203/23: Double or multiple optical cladding profiles
- C03B 2207/20: Specific substances in specified ports, e.g. all gas flows specified
- C03B 2207/50: Multiple burner arrangements
- C03B 2207/62: Distance
- C03B 2207/64: Angle
- C03B 2207/81: Constructional details of the feed line, e.g. heating, insulation, material, manifolds, filters
- G02B 6/036: core or cladding comprising multiple layers {(multicore optical fibres G02B6/02042; microstructured properties G02B6/02295; omniguide fibres G02B6/023)}
- C03B: MANUFACTURE, SHAPING, OR SUPPLEMENTARY PROCESSES
- G02B: OPTICAL ELEMENTS, SYSTEMS OR APPARATUS

## Abstract

This invention provides a manufacturing method for an optical fiber. In this invention, when the core layer loose body and the cladding layer loose body are deposited, the oxyhydrogen flame is used make a temperature of an interface between the core layer and the cladding layer rise, such that silicon dioxide at the interface appropriately contracts to form an isolation layer with a relatively high density. In addition, in this invention, a hollow glass tube is used as a target rod, and the hollow glass tube which is the target rod is directly connected with the core layer loose body. During the subsequent dehydration, not only a dehydration atmosphere penetrates from the outside to the inside of the cladding layer loose body, but also the dehydration atmosphere directly enters the core layer through the hollow glass tube.

## Claims

### Claim 1

A manufacturing method for an optical fiber, comprising the following steps:
A) using a hollow glass tube as a target rod, adopting a vapor phase axial deposition (VAD) method to manufacture a core rod loose body with a core layer loose body, a silicon dioxide isolation layer, and a cladding layer loose body sequentially arranged from inside out, and using a first blowtorch, a second blowtorch, and a third blowtorch for deposition, wherein gases entering the first blowtorch are H2, O2, Ar, and SiCl4, and the core layer loose body is formed; wherein gases entering the second blowtorch are H2 and O2, the silicon dioxide isolation layer is formed, a flow rate of H2 entering the second blowtorch is in a range of 12-15 L/min, and a flow rate of O2 entering the second blowtorch is in a range of 10-12 L/min; gases entering the third blowtorch are H2, O2, Ar, SiCl4, and CF4, and the cladding layer loose body is formed; and wherein the hollow glass tube comprises a hollow tube body and an open deposition tip communicating with a tail end of the hollow tube body, and the core layer loose body is connected with the open deposition tip;
B) dehydrating the core rod loose body, wherein a dehydration atmosphere enters the core layer loose body through the hollow glass tube and penetrates from an outside to an inside of the cladding layer loose body, and a dehydrated core rod loose body is obtained;
C) sequentially sintering, extending, and washing corrosively the dehydrated core rod loose body and forming an outer cladding layer on a surface to obtain a preform; and
D) drawing the preform to obtain an optical fiber.

### Claim 2 (depends on 1)

The manufacturing method according to claim 1, wherein the first blowtorch, the second blowtorch, and the third blowtorch are sequentially arranged from bottom to top.

### Claim 3 (depends on 1)

The manufacturing method according to claim 1, wherein the first blowtorch and the second blowtorch are arranged in parallel, an angle between the first blowtorch and a horizontal plane is in a range of 38°-50°, and an angle between the third blowtorch and the horizontal plane is in a range of 35°-45°.

### Claim 4 (depends on 1)

The manufacturing method according to claim 1, wherein a flame length from a blowtorch mouth of the first blowtorch to the core rod loose body is in a range of 40-50 mm; a flame length from a blowtorch mouth of the second blowtorch to the core rod loose body is in a range of 80-90 mm; and a flame length from a blowtorch mouth of the third blowtorch to the core rod loose body is in a range of 120-160 mm.

### Claim 5 (depends on 1)

The manufacturing method according to claim 1, wherein a distance between a center point of a blowtorch mouth of the first blowtorch and a center point of a blowtorch mouth of the second blowtorch is in a range of 70-80 mm, and a distance between the center point of the blowtorch mouth of the second blowtorch and a center point of a blowtorch mouth of the third blowtorch is in a range of 100-130 mm.

### Claim 6 (depends on 1)

The manufacturing method according to claim 1, wherein the first blowtorch comprises a raw material supply pipe located at a center of the first blowtorch for supplying a mixed gas of oxygen and SiCl4 and a seven-layer gas flow path concentrically arranged outside the raw material supply pipe, hydrogen, hydrogen, argon, oxygen, argon, hydrogen, and argon sequentially enter the seven-layer gas flow path from the center to an outside of the first blowtorch, a flow rate of the oxygen entering the raw material supply pipe is in a range of 13-15 L/min, and a flow rate of SiCl4 is in a range of 2-3 g/min; and flow rates of gases entering the seven-layer gas flow path are sequentially in ranges of 0.2-0.5 L/min, 2-4 L/min, 2-3 L/min, 15-17 L/min, 3-4 L/min, 13-17 L/min, and 4-5 L/min from the center to the outside of the first blowtorch;
the second blowtorch comprises a pipe located at a center of the second blowtorch for supplying hydrogen and a pipe for supplying oxygen arranged in a shape of a concentric circle outside the pipe for supplying the hydrogen;
the third blowtorch comprises a raw material supply pipe located at a center of the third blowtorch for supplying a mixed gas of oxygen and SiCl4 and a seven-layer gas flow path concentrically arranged outside the raw material supply pipe, hydrogen, hydrogen, a mixed gas of argon and CF4, oxygen, argon, hydrogen, and argon sequentially enter the seven-layer gas flow path from the center to an outside of the third blowtorch, a flow rate of the oxygen entering the raw material supply pipe is in a range of 25-27 L/min, a flow rate of SiCl4 is in a range of 15-25 g/min, and flow rates of gases entering the seven-layer gas flow path are sequentially in ranges of 2-3 L/min, 3-5 L/min, 3-7 L/min, 35-40 L/min, 4-5 L/min, 35-45 L/min, and 6-7 L/min from the center to the outside of the third blowtorch, wherein a total flow rate of the mixed gas of argon and CF4 is in a range of 3-7 L/min, a flow rate of argon is in a range of 2-3 L/min, and a flow rate of CF4 is in a range of 1-4 L/min; and
the open deposition tip is conical, a length of the open deposition tip is in a range of 20-22 mm, a hole with a diameter in a range of 6-7 mm is provided at the open deposition tip, an inner diameter of the hollow tube body is in a range of 30-31 mm, and an outer diameter of the hollow tube body is in a range of 32-34 mm.

### Claim 7 (depends on 1)

The manufacturing method according to claim 1, wherein the dehydration atmosphere is composed of helium and chlorine, and in the dehydration atmosphere, a content of the chlorine is in a range of 4% to 8%.

### Claim 8 (depends on 1)

The manufacturing method according to claim 1, wherein a pressure at which the dehydration atmosphere enters the core layer loose body through the hollow glass tube is in a range of 80-90 psi, and a pressure at which the dehydration atmosphere penetrates from an outside to an inside of the cladding layer loose body is in a range of 35-45 psi.

### Claim 9 (depends on 1)

The manufacturing method according to claim 1, wherein a dehydration temperature of the dehydrating in the step B) is in a range of 1245-1255° C.; and dehydration time of the dehydrating in the step B) is in a range of 2.5-3 hours.

### Claim 10 (depends on 1)

The manufacturing method according to claim 1, wherein when the core rod loose body is manufactured, a top end of the hollow tube body is sealed; and when the core rod loose body is dehydrated, the top end of the hollow tube body is open.

### Claim 11 (depends on 1)

The manufacturing method according to claim 1, wherein when the core rod loose body is manufactured, deposition starts on the hollow glass tube at a distance of 20 mm from a top end of the open deposition tip.

### Claim 12 (depends on 1)

The manufacturing method according to claim 1, wherein a deposition length of the core rod loose body manufactured by the VAD method is in a range of 500-1100 mm, and a deposition speed of the core rod loose body is in a range of 80-90 mm/h; and a diameter of the core layer loose body is in a range of 23.8-24.3 mm, a thickness of the silicon dioxide isolation layer is in a range of 0.8-1.2 mm, and a thickness of the cladding layer loose body is in a range of 50-60 mm.

### Claim 13 (depends on 1)

The manufacturing method according to claim 1, wherein a density of the core layer loose body is in a range of 0.2-0.25 g/cm3, a density of the silicon dioxide isolation layer is in a range of 0.9-1.13 g/cm3, and a density of the cladding layer loose body is in a range of 0.28-0.33 g/cm3.

### Claim 14 (depends on 1)

The manufacturing method according to claim 1, wherein a furnace temperature of drawing is in a range of 1950-2050° C., tension of the drawing is in a range of 100-230 g, a linear velocity of the drawing is in a range of 980-1050 m/min, and a length of the optical fiber after being drawn is in a range of 8-15 km.

### Claim 15 (depends on 1)

An optical fiber manufactured by the manufacturing method according to claim 1, wherein a loss of the optical fiber at a wavelength of 1550 nm is less than or equal to 0.172 dB/km, and a loss of the optical fiber at a wavelength of 1383 nm is less than or equal to 0.285 dB/km.

### Claim 16 (depends on 15)

The optical fiber according to claim 15, wherein the first blowtorch, the second blowtorch, and the third blowtorch are sequentially arranged from bottom to top.

### Claim 17 (depends on 15)

The optical fiber according to claim 15, wherein wherein the first blowtorch and the second blowtorch are arranged in parallel, an angle between the first blowtorch and a horizontal plane is in a range of 38°-50°, and an angle between the third blowtorch and the horizontal plane is in a range of 35°-45°.

### Claim 18 (depends on 15)

The optical fiber according to claim 15, wherein a flame length from a blowtorch mouth of the first blowtorch to the core rod loose body is in a range of 40-50 mm; a flame length from a blowtorch mouth of the second blowtorch to the core rod loose body is in a range of 80-90 mm; and a flame length from a blowtorch mouth of the third blowtorch to the core rod loose body is in a range of 120-160 mm.

### Claim 19 (depends on 15)

The optical fiber according to claim 15, wherein wherein a distance between a center point of a blowtorch mouth of the first blowtorch and a center point of a blowtorch mouth of the second blowtorch is in a range of 70-80 mm, and a distance between the center point of the blowtorch mouth of the second blowtorch and a center point of a blowtorch mouth of the third blowtorch is in a range of 100-130 mm.

### Claim 20 (depends on 15)

The optical fiber according to claim 15, wherein the first blowtorch comprises a raw material supply pipe located at a center of the first blowtorch for supplying a mixed gas of oxygen and SiCl4 and a seven-layer gas flow path concentrically arranged outside the raw material supply pipe, hydrogen, hydrogen, argon, oxygen, argon, hydrogen, and argon sequentially enter the seven-layer gas flow path from the center to an outside of the first blowtorch, a flow rate of the oxygen entering the raw material supply pipe is in a range of 13-15 L/min, and a flow rate of SiCl4 is in a range of 2-3 g/min; and flow rates of gases entering the seven-layer gas flow path are sequentially in ranges of 0.2-0.5 L/min, 2-4 L/min, 2-3 L/min, 15-17 L/min, 3-4 L/min, 13-17 L/min, and 4-5 L/min from the center to the outside of the first blowtorch;
the second blowtorch comprises a pipe located at a center of the second blowtorch for supplying hydrogen and a pipe for supplying oxygen arranged in a shape of a concentric circle outside the pipe for supplying the hydrogen;
the third blowtorch comprises a raw material supply pipe located at a center of the third blowtorch for supplying a mixed gas of oxygen and SiCl4 and a seven-layer gas flow path concentrically arranged outside the raw material supply pipe, hydrogen, hydrogen, a mixed gas of argon and CF4, oxygen, argon, hydrogen, and argon sequentially enter the seven-layer gas flow path from the center to an outside of the third blowtorch, a flow rate of the oxygen entering the raw material supply pipe is in a range of 25-27 L/min, a flow rate of SiCl4 is in a range of 15-25 g/min, and flow rates of gases entering the seven-layer gas flow path are sequentially in ranges of 2-3 L/min, 3-5 L/min, 3-7 L/min, 35-40 L/min, 4-5 L/min, 35-45 L/min, and 6-7 L/min from the center to the outside of the third blowtorch, wherein a total flow rate of the mixed gas of argon and CF4 is in a range of 3-7 L/min, a flow rate of argon is in a range of 2-3 L/min, and a flow rate of CF4 is in a range of 1-4 L/min; and
the open deposition tip is conical, a length of the open deposition tip is in a range of 20-22 mm, a hole with a diameter in a range of 6-7 mm is provided at the open deposition tip, an inner diameter of the hollow tube body is in a range of 30-31 mm, and an outer diameter of the hollow tube body is in a range of 32-34 mm.