# US 2020/0268487 A1 · Method for manufacturing zirconia slurry for forming porous surface on abutment and crown of ceramic implant and method for manufacturing implant using the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2020/0268487 A1
- Document ID: US20200268487A1
- Status: Published application
- Kind: A1
- Application number: 16/679,903
- Filed: 2019-11-11
- Published: 2020-08-27
- Earliest claimed: 2019-02-21
- Assignees: Dmax Co., Ltd.
- Applicants: Dmax Co., Ltd.
- Inventors: Tae Seok PARK
- Web page: https://patentgrep.com/patent/US20200268487A1

## CPC

- A61C 13/083: Porcelain or ceramic teeth {(A61C13/081 takes precedence; preparations A61K6/80)}
- A61C 5/73: Composite crowns
- A61C 5/77: Methods or devices for making crowns
- A61C 8/0012: {characterised by the material or composition, e.g. ceramics, surface layer, metal alloy (use of specific materials A61K6/00)}
- A61C 8/0013: {with a surface layer, coating}
- A61C 8/0048: {Connecting the upper structure to the implant, e.g. bridging bars (A61C8/0028 takes precedence)}
- A61C 13/00: Dental prostheses; Making same (tooth crowns for capping teeth A61C5/70; dental implants A61C8/00)
- A61C 13/0003: {Making bridge-work, inlays, implants or the like}
- A61K 6/802: comprising ceramics
- C04B 41/009: {characterised by the material treated}
- C04B 41/4582: {Porous coatings, e.g. coating containing porous fillers}
- C04B 41/52: Multiple coating or impregnating {multiple coating or impregnating with the same composition or with compositions only differing in the concentration of the constituents, is classified as single coating or impregnation}
- C04B 41/89: for obtaining at least two superposed coatings having different compositions
- A61C 5/20: Repairing attrition damage, e.g. facets
- C04B 2111/00836: {for medical or dental applications}
- A61C: DENTISTRY; APPARATUS OR METHODS FOR ORAL OR DENTAL HYGIENE (non-driven toothbrushes A46B; {tongue scrapers A61B17/24;} preparations for dentistry A61K6/00; preparations for cleaning the teeth or mouth A61K8/00, A61Q11/00)
- A61K: PREPARATIONS FOR MEDICAL, DENTAL OR TOILETRY PURPOSES (devices or methods specially adapted for bringing pharmaceutical products into particular physical or administering forms A61J3/00; chemical aspects of, or use of materials for deodorisation of air, for disinfection or sterilisation, or for bandages, dressings, absorbent pads or surgical articles A61L; soap compositions C11D)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE

## Abstract

The present invention relates to a method for manufacturing a zirconia slurry for forming porous surfaces on an abutment and a crown of a ceramic implant, the method including: the zirconia pulverization step (step S10) of putting zirconia powder, carbon powder as a foaming agent, and an organic binder in a ball mill and agitating and pulverizing the zirconia, carbon powder, and organic binder to allow the mixed zirconia powder to have nanoparticles; the carbon powder oxidization step (step S20) of heating the zirconia powder mixed with the carbon powder to a temperature of 1200 to 1800° C. and oxidizing the carbon powder to a concentration of 10 to 40 wt % to allow the porous surfaces to be formed on every particle of the zirconia powder; and the degreasing step (step S30) of putting a dispersing agent and a solvent in the zirconia powder whose particles have the porous surfaces to make a zirconia solution and removing the organic binder from the zirconia powder.

## Claims

### Claim 1

A method for manufacturing a zirconia slurry for forming porous surfaces on an abutment and a crown of a ceramic implant, the method comprising:
the zirconia pulverization step (step S10) of putting zirconia, carbon powder as a foaming agent, and an organic binder in a ball mill and agitating and pulverizing the zirconia, the carbon powder, and the organic binder to allow the zirconia mixture to have nanoparticles;
the carbon powder oxidization step (step S20) of heating the zirconia mixture mixed with the carbon powder to a temperature of 1200 to 1800° C. and oxidizing the carbon powder to a concentration of 10 to 40 wt % to allow the porous surfaces to be formed on every particle of the zirconia mixture; and
the degreasing step (step S30) of putting a dispersing agent and a solvent in the zirconia mixture having the porous surfaces to make a zirconia solution and removing the organic binder from to the zirconia mixture.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the zirconia pulverization step (step S10) comprises:
the powder preparation step (step S11) of selecting one from zirconium(IV) acetate hydroxide, zirconium nitrate, and zirconium chloride and pulverizing the selected zirconia material by means of the ball mill;
the distilled water preparation step (step S12) of adding double distilled water having a deionized process in an internal space of an autoclave used for hydrothermal synthesis; and
the powder dissolution step (step S13) of adjusting a temperature of the autoclave to which the distilled water is added to a temperature of 90 to 100° C., putting the zirconia powder and a precipitation agent into the autoclave, and dissolving the zirconia powder for two to four hours.

### Claim 3 (depends on 2)

The method according to claim 2, wherein the precipitation agent is one selected from NaOH and KOH.

### Claim 4 (depends on 1)

A method for manufacturing an implant with the zirconia slurry manufactured according to claim 1 so as to form porous surfaces on an abutment and a crown of the implant, the method comprising:
the slurry preparation step (S100) of putting the zirconia slurry in a storage container;
the component machining step (S200) of allowing an inner diameter of the crown to be more enlarged by 0.01 to 0.1 mm than a head of the abutment to ensure a spare space on a coupled surface between the crown and the abutment;
the slurry application step (S300) of applying the zirconia slurry to an inner periphery of the crown and the head of the abutment;
the slurry drying step (S400) of allowing the crown and the abutment to which the zirconia slurry is applied to be dried at a temperature of 120 to 150° C. for 10 to 20 minutes; and
the component coupling step (S500) of press-fitting the head of the abutment to the inner periphery of the crown to allow the abutment and the crown fitted to each other to be coupled to a fixture planted into a patient's alveolar bone.

### Claim 5 (depends on 1)

A method for manufacturing a laminate with the zirconia slurry manufactured according to claim 1, the method comprising:
the slurry preparation step (S100) of putting the zirconia slurry in a storage container;
the component machining step (S200) of putting a melted ceramic material into a mold to make a veneer;
the slurry application step (S300) of applying the zirconia slurry to an inner surface of the veneer;
the slurry drying step (S400) of allowing the veneer to which the zirconia slurry is applied to be dried at a temperature of 120 to 150° C. for 10 to 20 minutes; and
the component coupling step (S500) of applying a composite resin to a patient's tooth to attach the veneer to the tooth.

### Claim 6 (depends on 4)

The method according to claim 4, wherein the ball mill for pulverizing the zirconia powder comprises a machining container and at least one or more agitating balls (A) having different diameters disposed in the machining container, and the agitating balls (A) have porous surfaces to allow the zirconia powder to be machined to nanoparticles sizes.

### Claim 7 (depends on 5)

The method according to claim 5, wherein the ball mill for pulverizing the zirconia powder comprises a machining container and at least one or more agitating balls (A) having different diameters disposed in the machining container, and the agitating balls (A) have porous surfaces to allow the zirconia powder to be machined to nanoparticles sizes.

### Claim 8 (depends on 4)

The method according to claim 4, wherein at the slurry application step (S300), the zirconia slurry is applied toward a lower side of the crown from an inner upper periphery of the crown, thereby being enlargedly distributed toward the lower side of the crown from the inner upper periphery of the crown, and the zirconia slurry is applied toward the upper side of the abutment from the bottom of the head of the abutment, thereby being enlargedly distributed toward the upper side of the abutment from the bottom of the head of the abutment, so that the application flows of the zirconia slurry to the abutment and the crown are in reverse directions to each other.

### Claim 9 (depends on 5)

The method according to claim 5, wherein at the slurry application step (S300), the zirconia slurry is applied toward a lower side of the crown from an inner upper periphery of the crown, thereby being enlargedly distributed toward the lower side of the crown from the inner upper periphery of the crown, and the zirconia slurry is applied toward the upper side of the abutment from the bottom of the head of the abutment, thereby being enlargedly distributed toward the upper side of the abutment from the bottom of the head of the abutment, so that the application flows of the zirconia slurry to the abutment and the crown are in reverse directions to each other.