# US 2019/0376174 A1 · High Temperature Stable Compositionally Modulated Hard Coatings

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0376174 A1
- Document ID: US20190376174A1
- Status: Published application
- Kind: A1
- Application number: 16/485,384
- Filed: 2018-02-13
- Published: 2019-12-12
- Earliest claimed: 2017-02-13
- Assignees: Oerlikon Surface Solutions AG, PfäFfikon
- Applicants: Oerlikon Surface Solutions AG, PfäFfikon
- Inventors: Siva Phani Kumar YALAMANCHILI; Mirjam ARNDT; Juergen RAMM; Siegfried KRASSNITZER; Denis KURAPOV
- Web page: https://patentgrep.com/patent/US20190376174A1

## CPC

- C23C 14/0641: {Nitrides (C23C14/0617 takes precedence)}
- C23C 14/024: {Deposition of sublayers, e.g. to promote adhesion of the coating (C23C14/027 takes precedence)}
- C23C 14/3485: {using pulsed power to the target}
- C23C 30/005: {on hard metal substrates}
- C23C 14/35: by application of a magnetic field, e.g. magnetron sputtering {(C23C14/3457 takes precedence)}
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

The present invention relates to a component comprising a substrate coated with a coating having a film (3,4 or 3,4,5) comprising one or more transition metals, TM, aluminium, Al, and nitrogen, N, wherein the TM and N as well as Al and N are comprised in the film forming respectively nitride compounds, wherein the transition metal nitride, TM-N, is present in the film distributed in different portions exhibiting one crystalline phase of TM-N, and the aluminium nitride, Al—N, is present in the film in different portions exhibiting one phase of Al—N, whereas the phase of the transition metal nitride is cubic, c-TMN, the phase of the aluminium nitride is wurtzite, w-AIN, and wherein the film exhibits coherent or (semi-) coherent interfaces between the c-TMN phase portions and the w-AI-N phase portions.

## Claims

### Claim 1

Component comprising: a substrate coated with a coating having a film comprising one or more transition metals, TM, aluminium, Al, and nitrogen, N, wherein the TM and N as well as Al and N are comprised in the film forming respectively nitride compounds, wherein the transition metal nitride, TM-N, is present in the film distributed in different portions exhibiting one crystalline phase of TM-N, and the aluminium nitride, Al—N, is present in the film in different portions exhibiting one phase of Al—N,
characterized in that
the phase of the transition metal nitride is cubic, c-TMN,
the phase of the aluminium nitride is wurtzite, w-AlN,
and wherein the film exhibits coherent or (semi-) coherent interfaces between the c-TMN phase portions and the w-Al—N phase portions.

### Claim 2 (depends on 1)

Component of claim 1, wherein a compound with diffusion barrier properties is present at the interfaces between the c-TMN phase portions and the w-Al—N phase portions.

### Claim 3 (depends on 1)

Component of claim 1, wherein the substrate is a polycrystalline material and a seed layer is deposited between the substrate and the film.

### Claim 4 (depends on 1)

Component of claim 1, wherein the component is a tool, in particular a cutting tool.

### Claim 5

Hot work device in particular in the shape of a tool for milling or pressing in the shape of a polycrystalline substrate coated with a PVD hard coating exhibiting stability, in particular by exhibiting high hot hardness, in the temperature range between 800° C. and 1100° C.,
characterized in that
the said hard coating consists of
a seed layer in the shape of an w-AlN layer that is deposited directly on the polycrystalline substrate
followed by one single or at least one coating structure consisting of c-TMN and w-AlN phases with interfaces between the phases,

### Claim 6

Method for producing polycrystalline substrates coated with a PVD hard coating exhibiting stability, in particular by exhibiting high hot hardness, in the temperature range between 800° C. and 1100° C.
characterized in that
at first a seed layer in the shape of an w-AlN layer is deposited
that way that the seed layer exhibits a crystallographic orientation w-(0001), or w-(10-10), or w-(11-20)
and that after completion of the seed layer one single or at least one coating structure consisting of c-TMN and w-AlN phases with interfaces between the phases is deposited.

### Claim 7 (depends on 6)

Method of claim 6, wherein a coating structure consisting of c-TMN and w-AlN phases with interfaces between the phases forms the free surface of the coated substrate.

### Claim 8 (depends on 6)

Method of claim 6, wherein at least the deposition of the coating structure consisting of c-TMN and w-AlN phases is carried out by maintaining a substrate temperature of maximum 600° C., preferably around or ideally below 500° C.

### Claim 9 (depends on 6)

Method of claim 6, wherein the at least one coating structure consisting of c-TMN and w-AlN is a compositional and structural modulated coating.

### Claim 10 (depends on 6)

Method of claim 6, wherein the interfaces of the at least one coating structure consisting of c-TMN and w-AlN are self-adapted coherent and diffusion barrier interfaces between the phases.

### Claim 11 (depends on 6)

Method of claim 6, wherein the hardness H of the one coating structure or the outermost coating structure consisting of c-TMN and w-AlN phases is above 35 GPa at a temperature between 800° C. and 1100° C.

### Claim 12 (depends on 6)

Method of claim 6, wherein the coating structure consisting of c-TMN and w-AlN phases is a coating structure of c-TMN and w-AlN phases with a volume fraction between 70% and 100%.

### Claim 13 (depends on 6)

Method of claim 6, wherein the coating structure consisting of c-TMN and w-AlN phases is synthesized in a co-deposition method that way that the incident flux of TM and the incident flux of Al are co-deposited.

### Claim 14 (depends on 6)

Method of claim 6, wherein an adatom mobility above 50 nm/s is provided for at least during deposition of at least one coating structure consisting of c-TMN and w-AlN.

### Claim 15 (depends on 14)

Method of claim 14, wherein the said high adatom mobility is achieved by attaining a high plasma density which is preferably accomplished by using a HIPIMS deposition ideally using a power and/or current density higher than 750 W/cm2/0.8 A/cm2 or by combining such a HIPIMS deposition with an arc evaporation process.

### Claim 16 (depends on 14)

Method of claim 14, wherein the said high adatom mobility is achieved by applying an asymmetric bipolar pulsed bias at the substrate which preferably consists of a positive and a negative cycle.

### Claim 17 (depends on 14)

Method of claim 14, wherein the adatom mobility is enhanced by using surfactants such as or preferably in the shape of In, H2 and a combination of them, preferably in a proportion between 0.1 and 5% of the incident flux volume.

### Claim 18 (depends on 6)

Method of claim 6, wherein the c-TMN domains formed and/or the w-AlN domains formed have a size between 5 nm and 20 nm.

### Claim 19 (depends on 6)

Method of claim 6, wherein the structure comprised of c-TMN and w-AlN domains exhibits an interface material volume up to 50%.

### Claim 20 (depends on 6)

Method of claim 6, wherein a self-adapted diffusion barrier layer consisting of SiN, BN and/or WN is provided at the interfaces between the c-TMN and w-AlN domains, preferably with a thickness between 1 monolayer and 5 monolayers.

### Claim 21 (depends on 6)