# US 2019/0319117 A1 · Method and structure of fabricating i-shaped silicon germanium vertical field-effect transistors

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0319117 A1
- Document ID: US20190319117A1
- Status: Published application
- Kind: A1
- Application number: 15/954,843
- Filed: 2018-04-17
- Published: 2019-10-17
- Earliest claimed: 2018-04-17
- Assignees: International Business Machines Corporation
- Applicants: International Business Machines Corporation
- Inventors: ChoongHyun Lee; Kangguo Cheng; Juntao Li; Peng Xu
- Web page: https://patentgrep.com/patent/US20190319117A1

## CPC

- H10D 30/025: {of vertical IGFETs (of VDMOS H10D30/0291; of vertical TFTs H10D30/0318)}
- H10D 30/63: Vertical IGFETs (H10D30/66 {, H10D30/6728, H10D30/689, H10D30/693} take precedence)
- H10D 62/151: {of IGFETs (of IGFETs having LDD or DDD structure H10D30/601; of thin film transistors H10D30/6713)}
- H10D 62/292: {Non-planar channels of IGFETs (resulting from the gate electrode dispositions, e.g. within trenches H10D64/512)}
- H10D 62/314: {having vertical doping variations (vertical IGFETs H10D30/63)}
- H10D 62/822: comprising only Group IV materials heterojunctions, e.g. Si/Ge heterojunctions
- H10D 62/832: being Group IV materials comprising two or more elements, e.g. SiGe
- H10P 32/14: within a single semiconductor body or layer in a solid phase; between different semiconductor bodies or layers, both in a solid phase
- H10P 32/171: {being group IV material}
- H10P 50/642: {Chemical etching}
- H10P 50/692: {characterised by their composition, e.g. multilayer masks or materials}
- H10P 50/693: {characterised by their size, orientation, disposition, behaviour or shape, in horizontal or vertical plane}
- H10P 50/694: {characterised by their behaviour during the process, e.g. soluble masks or redeposited masks}
- H10P 50/695: {characterised by the process involved to create the mask, e.g. lift-off masks or sidewalls or to modify the mask}
- H10P 95/90: Thermal treatments, e.g. annealing or sintering
- H10D: INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10

## Abstract

A method for manufacturing a semiconductor device includes forming a first semiconductor layer having a first concentration of germanium on a semiconductor substrate, a second semiconductor layer having a second concentration of germanium on the first semiconductor layer, and a third semiconductor layer having a third concentration of germanium on the second semiconductor layer. The method also includes patterning the first, second and third semiconductor layers into at least one fin, and reducing a width of the second semiconductor layer of the at least one fin. In the method, a bottom source/drain region is grown from the substrate adjacent a base portion of the at least one fin, a gate structure is formed on and around the second semiconductor layer, and a top source/drain region is grown from the third semiconductor layer.

## Claims

### Claim 1

A method for manufacturing a semiconductor device, comprising:
forming a first semiconductor layer comprising a first concentration of germanium on a semiconductor substrate;
forming a second semiconductor layer comprising a second concentration of germanium on the first semiconductor layer;
forming a third semiconductor layer comprising a third concentration of germanium on the second semiconductor layer;
patterning the first, second and third semiconductor layers into at least one fin;
reducing a width of the second semiconductor layer of the at least one fin;
growing a bottom source/drain region from the substrate adjacent a base portion of the at least one fin;
forming a gate structure on and around the second semiconductor layer; and
growing a top source/drain region from the third semiconductor layer.

### Claim 2 (depends on 1)

The method according to claim 1, further comprising selectively forming a plurality of oxide mask layers on sides of the first and third semiconductor layers to mask the first and third semiconductor layers during a process to reduce the width of the second semiconductor layer of the at least one fin.

### Claim 3 (depends on 2)

The method according to claim 2, wherein selectively forming the plurality of oxide mask layers comprises:
forming a first germanium oxide layer on the substrate and the at least one fin;
performing a first annealing process to convert the first germanium oxide layer formed on the third semiconductor layer into a first silicon oxide mask layer; and
removing remaining portions of the first germanium oxide layer from the at least one fin and the substrate.

### Claim 4 (depends on 3)

The method according to claim 3, wherein selectively forming the plurality of oxide mask layers further comprises:
forming a second germanium oxide layer on the substrate, on the at least one fin and on the first silicon oxide mask layer;
performing a second annealing process to convert the second germanium oxide layer formed on the second semiconductor layer into a second silicon oxide mask layer; and
removing remaining portions of the second germanium oxide layer from the at least one fin, the first silicon oxide mask layer and the substrate.

### Claim 5 (depends on 4)

The method according to claim 4, wherein the second germanium oxide layer is thinner than the first germanium oxide layer.

### Claim 6 (depends on 4)

The method according to claim 4, wherein the second annealing process is performed at a higher temperature than the first annealing process.

### Claim 7 (depends on 4)

The method according to claim 4, wherein selectively forming the plurality of oxide mask layers further comprises:
forming a third germanium oxide layer on the substrate, on the at least one fin and on the first and the second silicon oxide mask layers;
performing a third annealing process to convert the third germanium oxide layer formed on the third semiconductor layer into a third silicon oxide mask layer; and
removing remaining portions of the third germanium oxide layer from the at least one fin, the first and second silicon oxide mask layers and the substrate.

### Claim 8 (depends on 7)

The method according to claim 7, wherein the third germanium oxide layer is thicker than the second germanium oxide layer.

### Claim 9 (depends on 7)

The method according to claim 7, wherein the third annealing process is performed at a higher temperature than the first and second annealing processes.

### Claim 10 (depends on 1)

The method according to claim 1, wherein the reducing of the width of the second semiconductor layer causes the first and third semiconductor layers to have a greater width than the second semiconductor layer.

### Claim 11 (depends on 1)

The method according to claim 1, wherein the first concentration of germanium is greater than the second concentration of germanium.

### Claim 12 (depends on 1)

The method according to claim 1, wherein the first concentration of germanium is greater than the third concentration of germanium.

### Claim 13 (depends on 1)

The method according to claim 1, wherein the second concentration of germanium is greater than the third concentration of germanium.

### Claim 14 (depends on 1)

The method according to claim 1, wherein the first, second and third semiconductor layers comprise silicon germanium.

### Claim 15 (depends on 1)

The method according to claim 1, further comprising performing junction annealing processes following the growing of the bottom and top source/drain regions.

### Claim 16

A vertical field-effect transistor device, comprising:
at least one fin disposed on a semiconductor substrate, wherein the at least one fin comprises:
a first semiconductor layer comprising a first concentration of germanium;
a second semiconductor layer comprising a second concentration of germanium disposed on the first semiconductor layer; and
a third semiconductor layer comprising a third concentration of germanium disposed on the second semiconductor layer;
wherein the first and third semiconductor layers have a greater width than the second semiconductor layer;
a bottom source/drain region adjacent a lower portion of the at least one fin;
a gate structure on the bottom source/drain region; and
a top source/drain region extending from the third semiconductor layer;
wherein the first concentration of germanium is greater than the second concentration of germanium.

### Claim 17

(canceled)

### Claim 18 (depends on 16)

The vertical field-effect transistor device according to claim 16, wherein the first concentration of germanium is greater than the third concentration of germanium.

### Claim 19 (depends on 16)

The vertical field-effect transistor device according to claim 16, wherein the second concentration of germanium is greater than the third concentration of germanium.

### Claim 20

A method for manufacturing a vertical field-effect transistor, comprising:
forming a first silicon germanium layer comprising a first concentration of germanium on a semiconductor substrate;
forming a second silicon germanium layer comprising a second concentration of germanium on the first silicon germanium layer;
forming a third silicon germanium layer comprising a third concentration of germanium on the second silicon germanium layer;
patterning the first, second and third silicon germanium layers into at least one fin;
reducing a width of the second silicon germanium layer of the at least one fin;
growing a bottom source/drain region from the substrate adjacent a base portion of the at least one fin;
forming a gate structure on and around the second silicon germanium layer; and
growing a top source/drain region from the third silicon germanium layer.