# US 2019/0316269 A1 · Method for ceramization of aluminum alloy surface

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0316269 A1
- Document ID: US20190316269A1
- Status: Published application
- Kind: A1
- Application number: 16/266,857
- Filed: 2019-02-04
- Published: 2019-10-17
- Earliest claimed: 2018-04-12
- Assignees: CITIC Dicastal Co., Ltd.
- Applicants: Citic Dicastal Co., Ltd
- Inventors: Deyu Han
- Web page: https://patentgrep.com/patent/US20190316269A1

## CPC

- C25D 9/06: by anodic processes
- C25D 11/08: containing inorganic acids
- C25D 5/44: Aluminium
- C25D 11/16: Pretreatment {, e.g. desmutting}
- C25D 11/24: Chemical after-treatment
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

The present invention provides a method for ceramization of an aluminum alloy surface, comprising the steps of: (1) providing a clean aluminum alloy surface; (2) pre-polishing; (3) etching; (4) polishing; and (5) performing ceramic oxidation. The advantages of the method are as follows: (1) good corrosion resistance, good elasticity and insulation; (2) the coating being similar to plastic, with enamel-like luster and attractive appearance; and (3) good adsorption capacity, capability of being dyed with different colors, and good decorative effect etc.

## Claims

### Claim 1

A method for ceramization of an aluminum alloy surface, comprising the steps of:
(1) providing a clean aluminum alloy surface;
(2) pre-polishing: rinsing the aluminum alloy surface obtained in step 1 in concentrated nitric acid for 1-5 minutes, followed by washing, the concentrated nitric acid being 380-400 g/L;
(3) etching: rinsing the aluminum alloy surface obtained in step 2 in an etching solution for 1-5 minutes, followed by washing, the etching solution containing 45-50 g/L of sodium hydroxide and 45-50 g/L of sodium fluoride, and the temperature being 60-70° C.;
(4) polishing: rinsing the aluminum alloy surface obtained in step 3 in concentrated nitric acid for 1-5 minutes, followed by washing, the concentrated nitric acid being 380-400 g/L; and
(5) performing ceramic oxidation: electroplating the aluminum alloy surface in a ceramic oxidation solution for 45-48 minutes, followed by washing, the aluminum alloy surface being an anode, a current density of the anode being 0.5-1.0 A/dm2, a voltage being 28-38V and a temperature being 45-50° C., and the ceramic oxidation solution comprising 36-38 g/L of chromic anhydride and 6-11 g/L of oxalic acid.

### Claim 2 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, wherein in step 1, the clean aluminum alloy surface is obtained by the following method:
(1A) rinsing with an alkaline solution without sodium hydroxide at 25-35° C. for 15-20 minutes, and
(1B) hot water washing followed by cold water washing.

### Claim 3 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, wherein in step 2, the aluminum alloy surface obtained in step 1 is rinsed in concentrated nitric acid for 4 minutes, and then washed, the concentrated nitric acid is 390 g/L.

### Claim 4 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, wherein in step 3, the aluminum alloy surface obtained in step 2 is rinsed in an etching solution for 4 minutes, and then washed, the etching solution contains 47 g/L of sodium hydroxide and 47 g/L of sodium fluoride, and the temperature is 65° C.

### Claim 5 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, wherein after step 3, hot water washing is followed by cold water washing; the hot water washing is performed 1-5 minutes, and a water temperature is 60-80° C.; the cold water washing is performed 1-5 minutes, and a water temperature is 15-20° C.

### Claim 6 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, wherein in step 4, the aluminum alloy surface obtained in step 3 is rinsed in concentrated nitric acid for 4 minutes, and then washed, the concentrated nitric acid is 390 g/L.

### Claim 7 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, further comprising a step of rinsing the aluminum alloy surface under a high pressure water gun between steps 4 and 5, a water pressure of the high pressure water gun is 1200-1400 Bar and a rinsing time is 30-60 seconds.

### Claim 8 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, wherein in step 5, the aluminum alloy surface is electroplated in a ceramic oxidation solution for 46 minutes, and then washed and dyed, the aluminum alloy surface is an anode, a current density of the anode is 0.72 A/dm2, a voltage is 32V and a temperature is 47° C.

### Claim 9 (depends on 1)

The method for ceramization of an aluminum alloy surface according to claim 1, further comprising step 6 of dyeing the aluminum alloy surface obtained in step 5 with a dye after step 5.

### Claim 10 (depends on 9)

The method for ceramization of an aluminum alloy surface according to claim 9, wherein the step of dyeing is selected from the group consisting of:
(6A) dyeing at 25-35° C. for 6-8 minutes using a blue dyeing solution containing 12-48 g/L of potassium ferrocyanide and 25-80 g/L of potassium chloride;
(6B) dyeing at 20-25° C. for 6-8 minutes using a black dyeing solution containing 55-85 g/L of cobalt acetate and 20-25 g/L of potassium permanganate; and
(6C) dyeing at 25-35° C. for 6-8 minutes using a white dyeing solution containing 10-50 g/L of lead acetate and 20-40 g/L of sodium sulfate.