# US 2019/0316242 A1 · Gradient Control Method for Microstructure Ultrafine Crystallization of Deep Cone Copper Shaped Charge Liner

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0316242 A1
- Document ID: US20190316242A1
- Status: Published application
- Kind: A1
- Application number: 16/292,361
- Filed: 2019-03-05
- Published: 2019-10-17
- Earliest claimed: 2018-04-16
- Assignees: No.59 Research Institute of China Ordnance Industry
- Applicants: No.59 Research Institute of China Ordnance Industry
- Inventors: Qiang CHEN; Dayu SHU; Qiang ZHAO; Zude ZHAO; Luchang CHE; Yang WU; Chuankai HU; Hui LI
- Web page: https://patentgrep.com/patent/US20190316242A1

## CPC

- C22F 1/08: of copper or alloys based thereon
- F42B 1/036: Manufacturing processes therefor {(F42B33/0214 - F42B33/0292 take precedence)}
- F42B 1/032: characterised by the material of the liner
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- F42B: EXPLOSIVE CHARGES, e.g. FOR BLASTING, FIREWORKS, AMMUNITION (explosive compositions C06B; fuzes F42C; blasting F42D)

## Abstract

A gradient control method for a microstructure ultrafine crystallization of a deep cone copper shaped charge liner includes the steps of an extrusion forming, a recrystallization heat treatment, and a high-frequency percussion. A multi-pass extrusion is used in the extrusion forming, and in the high-frequency percussion step, a percussion speed is 30,000 to 40,000 times/min, a percussion force is 1600 N to 2000 N, and a number of percussion times is 1 to 3. The forming and surface quality control of the deep cone shaped charge liner are realized by the control technology of the present invention; the plasticity of the material is improved, and fine crystal structures are obtained; and an ultrafine grain gradient structure distributed along the thickness direction is formed in the inner surface of the shaped charge liner.

## Claims

### Claim 1

A gradient control method for a microstructure ultrafine crystallization of a deep cone copper shaped charge liner, comprising steps of an extrusion forming, a recrystallization heat treatment, and a high-frequency percussion gradient;
wherein a multi-pass extrusion forming is used in the step of the extrusion forming, and in the step of the high-frequency percussion gradient, a percussion speed is 30,000 times/min to 40,000 times/min, a percussion force is 1600 N to 2000 N, and a number of percussion times is 1 to 3.

### Claim 2 (depends on 1)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 1, wherein the multi-pass extrusion forming is 4 to 8 passes of extrusion deformation under actions of a three-dimensional compressive stress and a deformation rate of 2 mm/s to 5 mm/s, a deformation amount of each pass of the 4 to 8 passes of extrusion deformation is 5% to 30%.

### Claim 3 (depends on 1)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 1, wherein the recrystallization heat treatment is carried out in a vacuum heat treatment furnace, a temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., a holding time of the recrystallization heat treatment is 45 min to 75 min.

### Claim 4 (depends on 1)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 1, wherein an annealing treatment is performed before the extrusion forming, an annealing temperature is 400° C. to 450° C., an annealing time is 1.5 h to 2 h, and then cooling to below 100° C. with a vacuum heat treatment furnace is performed, a vacuum degree of the vacuum heat treatment furnace is more than or equal to 2×10−3 Pa.

### Claim 5 (depends on 1)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 1, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, and a diameter of the copper rod is ϕ60 mm to 90 mm; the first billet is put into a vacuum heat treatment furnace to perform an annealing treatment, an annealing temperature is 400° C. to 450° C., annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×10−3 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under action of a three-dimensional compressive stress and a deformation rate of 2 mm/s to 5 mm/s, 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and a deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, a temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.

### Claim 6 (depends on 2)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 2, wherein the recrystallization heat treatment is carried out in a vacuum heat treatment furnace, a temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., a holding time of the recrystallization heat treatment is 45 min to 75 min.

### Claim 7 (depends on 2)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 2, wherein an annealing treatment is performed before the extrusion forming, an annealing temperature is 400° C. to 450° C., an annealing time is 1.5 h to 2 h, and then cooling to below 100° C. with a vacuum heat treatment furnace is performed, a vacuum degree of the vacuum heat treatment furnace is more than or equal to 2×10−3 Pa.

### Claim 8 (depends on 3)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 3, wherein an annealing treatment is performed before the extrusion forming, an annealing temperature is 400° C. to 450° C., an annealing time is 1.5 h to 2 h, and then cooling to below 100° C. with the vacuum heat treatment furnace is performed, a vacuum degree of the vacuum heat treatment furnace is more than or equal to 2×10−3 Pa.

### Claim 9 (depends on 2)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 2, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, a diameter of the copper rod is ϕ60 mm to 90 mm, and a material designation of the copper rod is chosen from the group of TU1, TU2, T2, T3; the first billet is put into a vacuum heat treatment furnace to perform an annealing treatment, an annealing temperature is 400° C. to 450° C., annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×10−3 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under the actions of the three-dimensional compressive stress and the deformation rate of 2 mm/s to 5 mm/s, the 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and the deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, a temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.

### Claim 10 (depends on 3)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 3, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, a diameter of the copper rod is ϕ60 mm to 90 mm, and a material designation of the copper rod is chosen from the group of TU1, TU2, T2, T3; the first billet is put into the vacuum heat treatment furnace to perform an annealing treatment, an annealing temperature is 400° C. to 450° C., annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×10−3 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under the actions of the three-dimensional compressive stress and the deformation rate of 2 mm/s to 5 mm/s, the 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and the deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, the temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and the holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.

### Claim 11 (depends on 4)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 4, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, a diameter of the copper rod is ϕ60 mm to 90 mm, and a material designation of the copper rod is chosen from the group of TU1, TU2, T2, T3; the first billet is put into the vacuum heat treatment furnace to perform the annealing treatment, the annealing temperature is 400° C. to 450° C., the annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×10−3 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under the actions of the three-dimensional compressive stress and the deformation rate of 2 mm/s to 5 mm/s, the 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and the deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, the temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and the holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.

### Claim 12 (depends on 6)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 6, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, a diameter of the copper rod is ϕ60 mm to 90 mm, and a material designation of the copper rod is chosen from the group of TU1, TU2, T2, T3; the first billet is put into the vacuum heat treatment furnace to perform an annealing treatment, an annealing temperature is 400° C. to 450° C., annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×10−3 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under the actions of the three-dimensional compressive stress and the deformation rate of 2 mm/s to 5 mm/s, the 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and the deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, the temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and the holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.

### Claim 13 (depends on 7)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 7, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, a diameter of the copper rod is ϕ60 mm to 90 mm, and a material designation of the copper rod is chosen from the group of TU1, TU2, T2, T3; the first billet is put into the vacuum heat treatment furnace to perform the annealing treatment, the annealing temperature is 400° C. to 450° C., the annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×103 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under the actions of the three-dimensional compressive stress and the deformation rate of 2 mm/s to 5 mm/s, the 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and the deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, the temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and the holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.

### Claim 14 (depends on 8)

The gradient control method for the microstructure ultrafine crystallization of the deep cone copper shaped charge liner of claim 8, wherein the gradient control method comprises the following steps:
(1) preparation of a billet: a copper rod is selected to prepare a first billet, a diameter of the copper rod is 4) 60 mm to 90 mm, and a material designation of the copper rod is chosen from the group of TU1, TU2, T2, T3; the first billet is put into the vacuum heat treatment furnace to perform the annealing treatment, the annealing temperature is 400° C. to 450° C., the annealing time is 1.5 h to 2 h, and then the first billet is cooled to below 100° C. with the vacuum heat treatment furnace to obtain the billet, the vacuum degree of the vacuum heat treatment is more than or equal to 2×10−3 Pa;
(2) the multi-pass extrusion forming: the billet obtained in the step (1) is placed in a mould cavity of an extrusion die, under the actions of the three-dimensional compressive stress and the deformation rate of 2 mm/s to 5 mm/s, the 4 to 8 passes of extrusion deformation are performed to obtain a first deep cone copper shaped charge liner, and the deformation amount for each pass of the 4 to 8 passes of extrusion deformation is between 5% and 30%;
(3) the recrystallization heat treatment: the first deep cone copper shaped charge liner obtained in the step (2) is placed in the vacuum heat treatment furnace to obtain a second deep cone copper shaped charge liner, the temperature of the recrystallization heat treatment is kept at 180° C. to 220° C., and the holding time of the recrystallization heat treatment is 45 min to 75 min;
(4) the high-frequency percussion gradient: an inner surface grain refining treatment is performed on the second deep cone shaped charge liner obtained in the step (3) on a high-frequency vibration percussion device to obtain a third deep cone shaped charge liner, the percussion speed is 30,000 times/min to 40,000 times/min, the percussion force is 1600 N to 2000 N, and the number of percussion times is 1 to 3;
(5) fine shaping: the third deep cone shaped charge liner obtained in the step (4) is placed in the mould cavity of the extrusion die, under actions of a three-dimensional compressive stress and a deformation rate of 1 mm/s to 3 mm/s, 1 to 4 passes of the fine shaping are performed, and a deformation amount for each pass of the fine shaping is less than or equal to 2%.