# US 2019/0316235 A1 · High strength steel sheet having excellent high-temperature elongation characteristic, warm-pressed member, and manufacturing methods for the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0316235 A1
- Document ID: US20190316235A1
- Status: Published application
- Kind: A1
- Application number: 16/470,401
- Filed: 2017-12-12
- Published: 2019-10-17
- Earliest claimed: 2016-12-20
- Assignees: Posco
- Applicants: Posco
- Inventors: Je-Woong LEE; Sang-Ho HAN
- Web page: https://patentgrep.com/patent/US20190316235A1

## CPC

- C21D 9/46: for sheet metals
- C22C 38/04: containing manganese
- C21D 1/32: Soft annealing, e.g. spheroidising
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/18: containing chromium
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/12: Aluminium or alloys based thereon
- C21D 2211/003: Cementite
- C21D 2211/005: Ferrite
- C21D 2211/009: Pearlite
- C22C 2204/00: End product comprising different layers, coatings or parts of cermet
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

Provided is a high strength steel sheet having an excellent high-temperature elongation characteristic. The sheet includes, by weight %, 0.4-0.9% of C, 0.01-1.5% of Cr, 0.03% or less (exclusive of 0%) of P, 0.01% or less (exclusive of 0%) of S, 0.01% or less (exclusive of 0%) of N, 0.01% or less (exclusive of 0%) of sol. Al, and a balance of Fe and inevitable impurities, and comprises at least one among 2.1% or less (exclusive of 0%) of Mn and 1.6% or less (exclusive of 0%) of Si; the sheet has a microcrystalline structure including pearlite having an area fraction of 80% or more and ferrite having an area fraction of 20% or less; and the pearlite includes cementite having a major axis length of 200 nm or shorter.

## Claims

### Claim 1

A high strength steel sheet having excellent high-temperature elongation characteristics, comprising, by weight %:
carbon (C): 0.4 to 0.9%, chromium (Cr): 0.01 to 1.5%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.01% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), alkali-soluble aluminum (sol.Al): 0.1% or less (excluding 0%), and a balance of iron (Fe) and inevitable impurities, and comprising at least one among manganese (Mn): 2.1% or less (excluding 0%), and silicon (Si): 1.6% or less (excluding 0%),
wherein a microstructure comprises 80% or more of pearlite and 20% or less of ferrite by area fraction, and
the pearlite comprises cementite having a major axis length of 200 nm or shorter.

### Claim 2 (depends on 1)

The high strength steel sheet having the high temperature elongation characteristic of claim 1, wherein the steel sheet satisfies the following Relational Expression 1,
0.7≤C+Cr/2+Mn/3+Si/4≤3.0 Relational Expression 1:
where a symbol of each element represents a content of each element in weight %, and is calculated as 0 if not included.

### Claim 3 (depends on 1)

The high strength steel sheet having the high temperature elongation characteristic of claim 1, wherein the cementite of the pearlite has an N value of 60% or more according to the following Relational Expression 2,
N(%)=Nx/(Nx+Ny)*100 Relational Expression 2:
(in the above Relational Expression 2, Nx is the number of cementite whose major axis length is 200 nm or less, and Ny is the number of cementite whose major axis length exceeds 200 nm.

### Claim 4 (depends on 1)

The high strength steel sheet having the high temperature elongation characteristic of claim 1, wherein the steel sheet has a tensile strength of 1000 MPa or more and an elongation of 60% or more in a temperature range of 500° C. to Ac1+30° C.

### Claim 5 (depends on 1)

The high strength steel sheet having the high temperature elongation characteristic of claim 1, wherein the steel sheet further has one of an aluminum plated layer, a galvanized layer, and an alloyed galvanized layer on its surface.

### Claim 6

A manufacturing method of a high strength steel sheet having a high-temperature elongation characteristic comprising steps of, by weight %:
heating a slab including carbon (C): 0.4 to 0.9%, chromium (Cr): 0.01 to 1.5%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.01% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), alkali-soluble aluminum (sol.Al): 0.1% or less (excluding 0%), and a balance of iron (Fe) and inevitable impurities, and including at least one among manganese (Mn): 2.1% or less (excluding 0%), and silicon (Si): 1.6% or less (excluding 0%) to a temperature of 1100° C. to 1300° C.;
finishing hot rolling the heated slab to a temperature in a range of Ar3+10° to Ar3+90° C. to obtain a hot-rolled steel sheet;
coiling the hot-rolled steel sheet at a temperature in a range of 550° C. to 700° C.; and
cold rolling the hot-rolled steel sheet at a reduction rate of 40 to 80% to obtain a cold-rolled steel sheet.

### Claim 7 (depends on 6)

The manufacturing method of the high strength steel sheet having the high-temperature elongation characteristic of claim 6, wherein the slab satisfies the following Relational Expression 1,
0.7≤C+Cr/2+Mn/3+Si/4≤3.0 Relational Expression 1:
(in the above Relational Expression 1, a symbol of each element represents a content of each element in weight %, and is calculated as 0 if not included.)

### Claim 8 (depends on 6)

The manufacturing method of the high strength steel sheet having the high-temperature elongation characteristic of claim 6, further comprising a step of performing batch annealing at a temperature in a range of 200° C. to 700° C. after the step of coiling.

### Claim 9 (depends on 6)

The manufacturing method of the high strength steel sheet having the high-temperature elongation characteristic of claim 6, further comprising a step of performing continuous annealing or batch annealing the cold-rolled steel sheet at a temperature in a range of Ac1−70° C. to Ac1+70° C.

### Claim 10 (depends on 6)

The manufacturing method of the high strength steel sheet having the high-temperature elongation characteristic of claim 6, further comprising a step of plating the cold-rolled steel sheet.

### Claim 11 (depends on 10)

The manufacturing method of the high strength steel sheet having the high-temperature elongation characteristic of claim 10, further comprising a step of alloying-treating the plated cold-rolled steel sheet.

### Claim 12 (depends on 6)

The manufacturing method of the high strength steel sheet having the high-temperature elongation characteristic of claim 6, wherein the cold rolling is performed at room temperature.

### Claim 13

A warm-pressed member by wt %, comprising:
carbon (C): 0.4 to 0.9%, chromium (Cr): 0.01 to 1.5%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.01% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), alkali-soluble aluminum (sol.Al): 0.1% or less (excluding 0%), and a balance of iron (Fe) and inevitable impurities, and including at least one among manganese (Mn): 2.1% or less (excluding 0%), and silicon (Si): 1.6% or less (excluding 0%),
wherein a microstructure comprises 80% or more of pearlite and 20% or less of ferrite by area fraction, and
the cementite of the ferrite has an N value of 70% or more by the following Relational Expression 2,
N(%)=Nx/(Nx+Ny)*100 Relational Expression 2:
(in the above Relational Expression 2, Nx is the number of cementite whose major axis length is 200 nm or less, and Ny is the number of cementite whose major axis length exceeds 200 nm.)

### Claim 14 (depends on 13)

The warm-pressed member of claim 13, wherein the warm-pressed member satisfies the following Relational Expression 1,
0.7≤C+Cr/2+Mn/3+Si/4≤3.0 Relational Expression 1:
(in the above Relational Expression 1, a symbol of each element represents a content of each element in weight %, and is calculated as 0 if not included.)

### Claim 15 (depends on 13)

The warm-pressed member of claim 13, wherein the warm-pressed member is further provided with an aluminum plated layer on the surface thereof.

### Claim 16 (depends on 13)

The warm-pressed member of claim 13, wherein the warm-pressed member is further provided with a galvanized layer or an alloyed galvanized layer on the surface thereof, and a microcrack length in the member is 10 μm or less.

### Claim 17 (depends on 6)

A manufacturing method of a warm-pressed member, comprising, a step of:
heating a steel sheet manufactured by a manufacturing method according to claim 6, and then forming the steel sheet into a press in a temperature range of to 500° C. to Ac1+30° C.

### Claim 18 (depends on 17)

The manufacturing method of the warm-pressed member of claim 17, wherein the forming is performed at a strain rate of 0.001/s or more.