# US 2019/0292314 A1 · Pbs resin composition and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0292314 A1
- Document ID: US20190292314A1
- Status: Published application
- Kind: A1
- Application number: 16/317,648
- Filed: 2017-11-30
- Published: 2019-09-26
- Earliest claimed: 2016-12-20
- Assignees: Kingfa Sci. & Tech. Co., Ltd.
- Applicants: Kingfa Sci. & Tech. Co., Ltd.
- Inventors: Weiwei Wang; Zhimin Yuan; Tongmin Cai; Xianbo Huang; Xiangbin Zeng; Renxu Yuan; Zhilong Guo; Meijun Tang
- Web page: https://patentgrep.com/patent/US20190292314A1

## CPC

- C08G 63/16: Dicarboxylic acids and dihydroxy compounds
- C08G 63/78: Preparation processes
- C08K 5/0091: {Complexes with metal-heteroatom-bonds}
- C08K 5/10: Esters; Ether-esters
- C08K 5/521: Esters of phosphoric acids, e.g. of H3PO4
- C08K 5/56: Organo-metallic compounds, i.e. organic compounds containing a metal-to-carbon bond
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)

## Abstract

The present invention discloses a PBS resin composition and a preparation method thereof. The composition comprises: a. PBS resin; b. element titanium; c. element phosphorus, wherein a weight ratio range of titanium to phosphorus is 0.6-10:1, preferably 0.7-4:1, and more preferably 1.25-1.5:1. A weight content of the element titanium is 20-200 ppm, and a weight content of the element phosphorus is 15-70 ppm. By adding a titanium-containing compound and a phosphorus-containing compound and controlling the range of the weight ratio of the element titanium to the element phosphorus in the PBS resin composition to be 0.6-10:1, the present invention obtains a PBS resin composition. After treating in a 95° C.-distilled water bath for 12 hours and drying at 90° C. for 3 hours, a change of the melt flow index of the PBS resin composition is less than 50.0 g/10 min, and the PBS resin composition possesses an obviously improved hydrolysis property.

## Claims

### Claim 1

A PBS resin composition, characterized in that, the PBS resin composition comprises following components:
a. PBS resin
b. element titanium
c. element phosphorus.

### Claim 2 (depends on 1)

The PBS resin composition according to claim 1, wherein a range of a weight ratio of the element titanium to the element phosphorus in the PBS resin composition is 0.6-10:1.

### Claim 3 (depends on 2)

The PBS resin composition according to claim 2, wherein the range of the weight ratio of the element titanium to the element phosphorus in the PBS resin composition is 0.7-4:1, and preferably 1.25-1.5:1.

### Claim 4 (depends on 1)

The PBS resin composition according to claim 1, wherein a weight content of the element titanium in the PBS resin composition is 20-200 ppm, and a weight content of the element phosphorus in the PBS resin composition is 15-70 ppm.

### Claim 5 (depends on 1)

The PBS resin composition according to claim 1, wherein with reference to the US EPA method 3052:1996 by using ICP-OES for analysis, the weight contents of the element titanium and the element phosphorus in the PBS resin composition are determined according to following procedure: weighing 0.1 g of the PBS resin composition and crushing, then dropping 5 mL of nitric acid to fully immerse the PBS resin composition; then dropping 1.0 mL of hydrogen peroxide to react for 2 minutes, sealing into a microwave digestion tank to digest at 210° C. for 3 hours; and after cooling to room temperature, filtering with a 0.45 μm filter membrane followed by diluting with distilled water to a volume of 50 mL for an ICP-OES test.

### Claim 6 (depends on 1)

The PBS resin composition according to claim 1, wherein the PBS resin composition has a melt flow index of 3.0-10.0 g/10 min when tested at 190° C. under a condition of 2.16 kg weight.

### Claim 7 (depends on 1)

The PBS resin composition according to claim 1, wherein said element titanium is from a titanium-containing compound, the titanium-containing compound being selected from one of or a mixture of more of N-butyl titanate and isopropyl titanate.

### Claim 8 (depends on 1)

The PBS resin composition according to claim 1, wherein said element phosphorus is from a phosphorus-containing compound, the phosphorus compound being selected from one of or a mixture of more of triethyl phosphate, trimethyl phosphate, tributyl phosphate and triphenyl phosphate.

### Claim 9 (depends on 1)

The PBS resin composition according to claim 1, wherein after treating in a 95° C.-distilled water bath for 12 hours and drying at 90° C. for 3 hours, a change of the melt flow index of the PBS resin composition is less than 50.0 g/10 min.

### Claim 10 (depends on 1)

A preparation method of the PBS resin composition according to claim 1, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 11 (depends on 2)

A preparation method of the PBS resin composition according to claim 2, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 12 (depends on 3)

A preparation method of the PBS resin composition according to claim 3, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 13 (depends on 4)

A preparation method of the PBS resin composition according to claim 4, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 14 (depends on 5)

A preparation method of the PBS resin composition according to claim 5, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 15 (depends on 6)

A preparation method of the PBS resin composition according to claim 6, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 16 (depends on 7)

A preparation method of the PBS resin composition according to claim 7, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.

### Claim 17 (depends on 8)

A preparation method of the PBS resin composition according to claim 8, characterized in that, the preparation method comprises the following steps:
S1. mixing succinic acid, 1,4-butanediol and a titanium-containing compound, and maintaining at a temperature of 180-250° C. under a pressure of 50-100 kPa for 1-5 hours;
S2. after aerating CO2, adding a phosphorus-containing compound and maintaining for 10-30 minutes; and
S3. reducing the pressure to less than 100 Pa, heating a mixture obtained in step 2 to 230-250° C., maintaining for 3-6 hours, aerating nitrogen and pelletizing.