# US 2019/0246497 A1 · Flexible substrate and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0246497 A1
- Document ID: US20190246497A1
- Status: Published application
- Kind: A1
- Application number: 15/761,099
- Filed: 2018-03-05
- Published: 2019-08-08
- Earliest claimed: 2018-02-07
- Assignees: Shenzhen China Star Optoelectronics Technology Co., Ltd.
- Applicants: Shenzhen China Star Optoelectronics Technology Co., Ltd.
- Inventors: Yu SHI; Lixuan CHEN
- Web page: https://patentgrep.com/patent/US20190246497A1

## CPC

- H10K 77/111: {Flexible substrates}
- G06F 1/1652: {the display being flexible, e.g. mimicking a sheet of paper, or rollable}
- G09F 9/301: {flexible foldable or roll-able electronic displays, e.g. thin LCD, OLED}
- H05K 1/0393: {Flexible materials (H05K1/038 takes precedence; specific organic compositions are classified in H05K1/0313 and subgroups)}
- H10K 59/873: {Encapsulations}
- H10K 59/879: {comprising refractive means, e.g. lenses}
- H10K 71/80: using temporary substrates
- H10W 90/00: Package configurations
- H05K 2201/0108: Transparent
- H05K 2201/0154: Polyimide
- H05K 2203/016: Temporary inorganic, non-metallic carrier, e.g. for processing or transferring
- Y02E 10/549: Organic PV cells
- H10K: ORGANIC ELECTRIC SOLID-STATE DEVICES
- G06F: ELECTRIC DIGITAL DATA PROCESSING (computer systems based on specific computational models G06N)
- G09F: DISPLAYING; ADVERTISING; SIGNS; LABELS OR NAME-PLATES; SEALS
- H05K: PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present disclosure provides a method for manufacturing a flexible substrate. The method includes forming at least two flexible substrate layers in a stacking form on a surface of a glass baseplate, wherein a first flexible substrate layer of the flexible substrate layers relatively close to the glass baseplate has a refractive index less than a refractive index of a second flexible substrate layer of the flexible substrate layers relatively far from the glass baseplate; forming a water and oxygen blocking layer on a surface of the second flexible substrate layers, wherein the water and oxygen blocking layer has a refractive index greater than the refractive index of the second flexible substrate layers disposed below the water and oxygen blocking layer.

## Claims

### Claim 1

A method for manufacturing a flexible substrate, comprising:
a step S10 of providing a glass baseplate;
a step S20 of forming at least two flexible substrate layers in a stacking form on a surface of the glass baseplate, wherein a first flexible substrate layer of the flexible substrate layers relatively close to the glass baseplate has a refractive index less than a refractive index of a second flexible substrate layer of the flexible substrate layers relatively far from the glass baseplate;
a step S30 of forming a water and oxygen blocking layer on a surface of the second flexible substrate layers, wherein the water and oxygen blocking layer has a refractive index greater than the refractive index of the second flexible substrate layers disposed below the water and oxygen blocking layer, and the water and oxygen blocking layer is made of a material selected from silicon nitride, aluminum oxide, titanium oxide, zirconia, or any combination thereof; and
a step S40 of removing the glass baseplate, such that the flexible substrate having a high transmittance is formed.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the flexible substrate layers are made of polyimide.

### Claim 3 (depends on 2)

The method according to claim 2, wherein the step S20 comprises:
a step S201 of forming a first polyimide layer on the surface of the glass baseplate; and
a step S202 of forming a second polyimide layer on a surface of the first polyimide layer.

### Claim 4 (depends on 3)

The method according to claim 3, wherein the step S201 comprises:
providing 4,4′-diaminodiphenyl ether as a diamine, and 4,4′-hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride as dianhydrides, and then dissolving 4,4′-diaminodiphenyl ether, 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride in N-methylpyrrolidone, so as to form a first polyamic acid solution containing 10-14% of fluorine, wherein a solid content of the first polyamic acid solution is 10-14%;
coating the first polyamic acid solution on the surface of the glass baseplate; and
heating a coating layer of the first polyamic acid solution, wherein a heating temperature is ramped up to 300-400° C. in accordance with a predetermined procedure, so as to cure the coating layer of the first polyamic acid solution to form the first polyimide layer; and
wherein the step S202 comprises:
dissolving 4,4′-(diphenylsulfonyl(4,1-bezene)disulfide)diphenylamine and 3,3′,4,4′-biphenyltetracarboxylic dianhydride of same moles in N-methylpyrrolidone so as to form a second polyamic acid solution, wherein a solid content of the second polyamic acid solution is 13-17%;
coating the second polyamic acid solution on a surface of the first polyimide layer; and
heating a coating layer of the second polyamic acid solution, wherein the heating temperature is ramped up to 300-350° C. in accordance with the predetermined procedure, so as to cure the coating layer of the second polyamic acid solution to form the second polyimide layer.

### Claim 5 (depends on 3)

The method according to claim 3, wherein the step S201 comprises:
providing 4,4′-diaminodiphenyl ether as a diamine, and 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride as dianhydrides, and then dissolving 4,4′-diaminodiphenyl ether, 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride in N-methylpyrrolidone, so as to form a first polyamic acid solution containing 10-14% of fluorine, wherein a solid content of the first polyamic acid solution is 10-14%;
coating the first polyamic acid solution on a surface of the glass baseplate; and
heating a coating layer of the first polyamic acid solution, wherein a heating temperature is ramped up to 300-400° C. in accordance with a predetermined procedure, so as to cure the coating layer of the first polyamic acid solution to form the first polyimide layer; and
wherein the step S202 comprises:
dissolving 9,9-bis(4-(4-amino-3-hydroxy)phenoxy)phenylfluorene and 4,4′-(hexafluoroisopropylidene)diplithalic anhydride of same moles in isoquinoline, so as to form a second polyamic acid solution, wherein the second polyamic acid solution includes polyamic acid and polyimide, and a solid content of the second polyamic acid solution is 13-17%; and then adding zirconium tetra-n-butoxy into the second polyamic acid solution, such that a ratio of polyimide to zirconium tetra-n-butoxy is 1:1.5;
coating the second polyamic acid solution on a surface of the first polyimide layer; and
heating a coating layer of the second polyamic acid solution, wherein the heating temperature is ramped up to 300-350° C. in accordance with the predetermined procedure, so as to cure the coating layer of the second polyamic acid solution to form the second polyimide layer.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the water and oxygen blocking layer is made of aluminum oxide having a low refractive index.

### Claim 7

A method for manufacturing a flexible substrate, comprising:
a step S10 of providing a glass baseplate;
a step S20 of forming at least two flexible substrate layers in a stacking form on a surface of the glass baseplate, wherein a first flexible substrate layer of the flexible substrate layers relatively close to the glass baseplate has a refractive index less than a refractive index of a second flexible substrate layer of the flexible substrate layers relatively far from the glass baseplate;
a step S30 of forming a water and oxygen blocking layer on a surface of the second flexible substrate layers, wherein the water and oxygen blocking layer has a refractive index greater than the refractive index of the second flexible substrate layers disposed below the water and oxygen blocking layer; and
a step S40 of removing the glass baseplate such that the flexible substrate having a high transmittance is formed.

### Claim 8 (depends on 7)

The method according to claim 7, wherein the flexible substrate layers are made of polyimide.

### Claim 9 (depends on 8)

The method according to claim 8, wherein the step S20 comprises:
a step S201 of forming a first polyimide layer on a surface the glass baseplate; and
a step S202 of forming a second polyimide layer on a surface of the first polyimide layer.

### Claim 10 (depends on 9)

The method according to claim 9, wherein the step S201 comprises:
providing 4,4′-diaminodiphenyl ether as a diamine, and 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride as dianhydrides, and then dissolving 4,4′-diaminodiphenyl ether, 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride in N-methylpyrrolidone, so as to form a first polyamic acid solution containing 10-14% of fluorine, wherein a solid content of the first polyamic acid solution is 10-14%;
coating the first polyamic acid solution on the surface of the glass baseplate; and
heating a coating layer of the first polyamic acid solution, wherein a heating temperature is ramped up to 300-400° C. in accordance with a predetermined procedure, so as to cure the coating layer of the first polyamic acid solution to form the first polyimide layer; and
wherein the step S202 comprises:
dissolving 4,4′-(diphenylsulfonyl(4,1-benzene)disulfide)diphenylamine and 3,3′,4,4′-biphenyltetracarboxylic dianhydride of same moles in N-methylpyrrolidone, so as to form a second polyamic acid solution, wherein a solid content of the second polyamic acid solution is 13-17%;
coating the second polyamic acid solution on a surface of the first polyimide layer; and
heating a coating layer of the second polyamic acid solution, wherein the heating temperature is ramped up to 300-350° C. in accordance with the predetermined procedure, so as to cure the coating layer of the second polyamic acid solution to form the second polyimide layer.

### Claim 11 (depends on 9)

The method according to claim 9, wherein the step S201 comprises:
providing 4,4′-diaminodiphenyl ether as a diamine, and 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride as dianhydrides, and then dissolving 4,4′-diaminodiphenyl ether, 4,4′-(hexafluoroisopropylidene)diphthalic anhydride and pyromellitic dianhydride in N-methylpyrrolidone, so as to form a first polyamic acid solution containing 10-14% of fluorine, wherein a solid content of the first polyamic acid solution is 10-14%;
coating the first polyamic acid solution on the surface of the glass baseplate; and
heating a coating layer of the first polyamic acid solution, wherein a heating temperature is ramped up to 300-400° C. in accordance with a predetermined procedure, so as to cure the coating layer of the first polyamic acid solution to form the first polyimide layer; and
wherein the step S202 comprises:
dissolving 9,9-bis(4-(4-amino-3-hydroxy)phenoxy)phenylfluorene and 4,4′-(hexafluoroisopropylidene)diphthalic anhydride of same moles in isoquinoline, so as to form a second polyamic acid solution, wherein the second polyamic acid solution includes polyamic acid and polyimide, and a solid content of the second polyamic acid solution is 13-17%; and then adding zirconium tetra-n-butoxy into the second polyamic acid solution, such that a ratio of polyimide to zirconium tetra-n-butoxy is 1:1.5;
coating the second polyamic acid solution on a surface of the first polyimide layer; and
heating a coating layer of the second polyamic acid solution, wherein the heating temperature is ramped up to 300-350° C. in accordance with the predetermined procedure, so as to cure the coating layer of the second polyamic acid solution to form the second polyimide layer.

### Claim 12

A flexible substrate, comprising:
a first flexible substrate layer;
a second flexible substrate layer disposed on a surface of the first flexible substrate layer; and
a water and oxygen blocking layer disposed on a surface of the second flexible substrate layer;
wherein the first flexible substrate layer is configured as a light-incident side of the flexible substrate, and the water and oxygen blocking layer is configured as a light-emitting side of the flexible substrate, and
wherein a refractive index of the first flexible substrate layer, a refractive index of the second flexible substrate layer, and a refractive index of the water and oxygen blocking layer are increased in turn.

### Claim 13 (depends on 12)

The flexible substrate according to claim 12, wherein the first flexible substrate layer and the second flexible substrate layer are made of polyimide.

### Claim 14 (depends on 12)

The flexible substrate according to claim 12, wherein the water and oxygen blocking layer is made of aluminum oxide having a low refractive index.