# US 2019/0194775 A1 · Steel sheet and method for producing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0194775 A1
- Document ID: US20190194775A1
- Status: Published application
- Kind: A1
- Application number: 16/329,672
- Filed: 2017-09-28
- Published: 2019-06-27
- Earliest claimed: 2016-09-28
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Yoshihiko ONO; Shimpei YOSHIOKA; Nobuyuki NAKAMURA; Hiroshi HASEGAWA
- Web page: https://patentgrep.com/patent/US20190194775A1

## CPC

- C21D 9/46: for sheet metals
- B32B 15/01: all layers being exclusively metallic {(making layered metal workpieces by pressure cladding B23K20/22; making coatings with a metallic material characterised by its composition C23C30/00)}
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- B32B 15/04: comprising metal as the main or only constituent of a layer, {which is} next to another layer of {the same or of} a {different material (next to a bituminous or tarry layer B32B11/08; next to a water-setting substance layer B32B13/06; next to a glass layer B32B17/061; next to a cellulosic plastic layer B32B23/042)}
- B32B 15/043: {of metal (B32B15/01 takes precedence)}
- B32B 15/18: comprising iron or steel {(B32B15/011, B32B15/012 and B32B15/013 take precedence)}
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/021: involving particular fabrication steps or treatments of ingots or slabs
- C21D 8/0236: {Cold rolling}
- C21D 8/0247: characterised by the heat treatment
- C21D 8/04: to produce plates or strips for drawing, e.g. for deep-drawing
- C21D 8/041: {involving a particular fabrication or treatment of ingot or slab}
- C21D 8/0426: {Hot rolling}
- C21D 8/0436: {Cold rolling}
- C21D 8/0473: {Final recrystallisation annealing}
- C21D 9/52: for wires; for strips {; for rods of unlimited length}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/18: containing chromium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/40: with nickel
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/54: with boron
- C22C 38/58: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/40: Plates; Strips
- C23C 28/025: {with at least one zinc-based layer}
- C23C 28/3225: {with at least one zinc-based layer}
- C23C 30/00: Coating with metallic material characterised only by the composition of the metallic material, i.e. not characterised by the coating process (C23C26/00, C23C28/00 take precedence)
- C23C 30/005: {on hard metal substrates}
- C21D 2211/002: Bainite
- C21D 2211/008: Martensite
- Y02P 10/20: Recycling
- Y10T 428/12757: Fe
- Y10T 428/12799: Next to Fe-base component [e.g., galvanized]
- Y10T 428/12951: Fe-base component
- Y10T 428/12972: Containing 0.01-1.7% carbon [i.e., steel]
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

A steel sheet having a specified chemical composition and a method for producing the steel sheet. The steel sheet has a microstructure including martensite and bainite. The total area fraction of the martensite and the bainite to the entirety of the microstructure is more than 90% and 100% or less. The microstructure includes inclusion clusters A and B, the content of the clusters A in the microstructure being 2 clusters/mm2 or less, and the content of the clusters B in the microstructure being 5 clusters/mm2 or less. The microstructure includes carbide particles including Fe as a main constituent which have an aspect ratio of 2.0 or less and a major axis of 0.30 μm or more and 2 μm or less. The content of the carbide particles in the microstructure is 4000 particles/mm2 or less. The microstructure includes prior γ grains having an average size of 6 to 15 μm.

## Claims

### Claim 1

A steel sheet having a chemical composition comprising, by mass %:
C: 0.13% to 0.40%,
Si: 1.5% or less,
Mn: 1.8% to 4%,
P: 0.02% or less,
S: less than 0.0010%,
sol. Al: 0.2% or less,
N: less than 0.0060%,
B: 0.0003% or more and less than 0.0035%, and
O: less than 0.0020%,
at least one of Nb: 0.002% or more and less than 0.035%, and Ti: 0.002% or more and less than 0.040%, and
the balance being Fe and inevitable impurities,
wherein the steel sheet has a microstructure including (i) martensite and bainite, a total area fraction of the martensite and the bainite to an entirety of the microstructure being in a range of more than 90% and 100% or less, (ii) prior-γ grains having an average grain size of 6 to 15 μm, (iii) inclusion clusters A having a major axis of 100 μm or more, each of the inclusion clusters A being constituted by one or more inclusion particles, the inclusion particles having a major axis of 0.3 μm or more, and, in the case where the inclusion clusters are constituted by two or more inclusion particles, a shortest distance between the inclusion particles is 30 μm or less, and inclusion clusters B having a major axis of 20 μm or more and less than 100 μm, each of the inclusion clusters B being constituted by one or more inclusion particles, the inclusion particles having a major axis of 0.3 μm or more, and, in the case where the inclusion clusters are constituted by two or more inclusion particles, a shortest distance between the inclusion particles is 10 μm or less, the content of the inclusion clusters A in the microstructure being 2 clusters/mm2 or less, and the content of the inclusion clusters B in the microstructure being 5 clusters/mm2 or less, and (iv) carbide particles including Fe as a main constituent, the carbide particles having an aspect ratio of 2.0 or less and a major axis of 0.30 μm or more and 2 μm or less, and the content of the carbide particles in the microstructure being 4000 particles/mm2 or less,
Formula (1) and Formula (2) are both satisfied:
[% Ti]+[% Nb]>0.007 (1)
[% Ti]×[% Nb]2<7.5×10−6 (2)
where [% Nb] and [% Ti] represent the contents (mass %) of Nb and Ti, respectively, and
the steel has a thickness of 0.5 to 2.6 mm and a tensile strength of 1320 MPa or more.

### Claim 2 (depends on 1)

The steel sheet according to claim 1, wherein carbide particles having a diameter of 10 to 200 nm are dispersed inside at least one of the martensite and the bainite, the content of the carbide particles in the at least one of the martensite and the bainite being 0.3×107 particles/mm2 or more.

### Claim 3 (depends on 1)

The steel sheet according to claim 1, wherein the microstructure includes retained γ, and the area fraction of the retained γ to the entirety of the microstructure is less than 5%.

### Claim 4 (depends on 1)

The steel sheet according to claim 1, the chemical composition further comprising, by mass %, at least one group selected from Groups A-D:
Group A: at least one of Cu: 0.005% to 1% and Ni: 0.01% to 1%.
Group B: at least one element selected from the group consisting of:
Cr: 0.01% to 1.0%,
Mo: 0.01% to 0.5%,
V: 0.003% to 0.5%,
Zr: 0.005% to 0.2%, and
W: 0.005% to 0.2%,
Group C: at least one element selected from the group consisting of:
Ca: 0.0002% to 0.0030%,
Ce: 0.0002% to 0.0030%,
La: 0.0002% to 0.0030%, and
Mg: 0.0002% to 0.0030%, and
Group D: at least one of Sb: 0.002% to 0.1%, and Sn: 0.002% to 0.1%.

### Claim at position 5

5-7. (canceled)

### Claim 8 (depends on 1)

The steel sheet according to claim 1, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 9 (depends on 1)

A method for producing a steel sheet, the method comprising:
soaking a steel slab having the chemical composition according to claim 1 for 100 minutes or more with a slab-heating temperature higher than 1220° C. and subsequently hot-rolling the steel slab into a hot-rolled steel sheet;
cold-rolling the hot-rolled steel sheet into a cold-rolled steel sheet at a rolling in a range of 20% to 75% such that the cold-rolled steel sheet has a thickness of 0.5 to 2.6 mm; and
performing annealing of the cold-rolled steel sheet, the annealing including soaking the cold-rolled steel sheet for in a range of 150 to 600 seconds at an annealing temperature in a range of 860° C. or more and 910° C. or less, subsequently cooling from the annealing temperature to 420° C. at an average cooling rate of 2° C./s or more, and further cooling from 420° C. to 280° C. or less at an average cooling rate of 10° C./s or more.

### Claim 10 (depends on 9)

The method for producing a steel sheet according to claim 9, wherein, in the annealing, subsequent to the cooling to 280° C. or less, reheating as needed, holding at a temperature in a range of 120° C. to 280° C. for in a range of 15 seconds to 3 days, and subsequently cooling to a room temperature.

### Claim 11 (depends on 9)

The method for producing a steel sheet according to claim 9, wherein, during cooling from the annealing temperature to 420° C. at an average cooling rate of 2° C./s or more in the annealing, the steel sheet is immersed in a plating bath in order to perform coating of the steel sheet.

### Claim 12 (depends on 11)

The method for producing a steel sheet according to claim 11, wherein, after the steel sheet has been immersed in the plating bath in the coating, the steel sheet is heated to a temperature in a range of 480° C. to 600° C. in order to perform alloying.

### Claim 13 (depends on 4)

The steel sheet according to claim 4, wherein carbide particles having a diameter of 10 to 200 nm are dispersed inside at least one of the martensite and the bainite, the content of the carbide particles in the at least one of the martensite and the bainite being 0.3×107 particles/mm2 or more.

### Claim 14 (depends on 2)

The steel sheet according to claim 2, wherein the microstructure includes retained γ, and the area fraction of the retained γ to the entirety of the microstructure is less than 5%.

### Claim 15 (depends on 4)

The steel sheet according to claim 4, wherein the microstructure includes retained γ, and the area fraction of the retained γ to the entirety of the microstructure is less than 5%.

### Claim 16 (depends on 13)

The steel sheet according to claim 13, wherein the microstructure includes retained γ, and the area fraction of the retained γ to the entirety of the microstructure is less than 5%.

### Claim 17 (depends on 2)

The steel sheet according to claim 2, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 18 (depends on 3)

The steel sheet according to claim 3, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 19 (depends on 4)

The steel sheet according to claim 4, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 20 (depends on 13)

The steel sheet according to claim 13, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 21 (depends on 14)

The steel sheet according to claim 14, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 22 (depends on 15)

The steel sheet according to claim 15, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 23 (depends on 16)

The steel sheet according to claim 16, wherein the steel sheet has a coating layer deposited on the surface thereof.

### Claim 24 (depends on 4)

A method for producing a steel sheet, the method comprising:
a steel slab having the chemical composition according to claim 4 for 100 minutes or more with a slab-heating temperature higher than 1220° C. and subsequently hot-rolling the steel slab into a hot-rolled steel sheet;
cold-rolling the hot-rolled steel sheet into a cold-rolled steel sheet at a rolling reduction in a range of 20% to 75% such that the cold-rolled steel sheet has a thickness of 0.5 to 2.6 mm; and
performing annealing of the cold-rolled steel sheet, the annealing including soaking the cold-rolled steel sheet for in a range of 150 to 600 seconds at an annealing temperature in a range of 860° C. or more and 910° C. or less, subsequently cooling from the annealing temperature to 420° C. at an average cooling rate of 2° C./s or more, and further cooling from 420° C. to 280° C. or less at an average cooling rate of 10° C./s or more.

### Claim 25 (depends on 24)

The method for producing a steel sheet according to claim 24, wherein, in the annealing, subsequent to the cooling to 280° C. or less, reheating as needed, holding at a temperature in a range of 120° C. to 280° C. for in a range of 15 seconds to 3 days, and subsequently cooling to a room temperature.

### Claim 26 (depends on 24)

The method for producing a steel sheet according to claim 24, wherein, during cooling from the annealing temperature to 420° C. at an average cooling rate of 2° C./s or more in the annealing, the steel sheet is immersed in a plating bath in order to perform coating of the steel sheet.

### Claim 27 (depends on 10)

The method for producing a steel sheet according to claim 10, wherein, during cooling from the annealing temperature to 420° C. at an average cooling rate of 2° C./s or more in the annealing, the steel sheet is immersed in a plating bath in order to perform coating of the steel sheet.

### Claim 28 (depends on 25)

The method for producing a steel sheet according to claim 25, wherein, during cooling from the annealing temperature to 420° C. at an average cooling rate of 2° C./s or more in the annealing, the steel sheet is immersed in a plating bath in order to perform coating of the steel sheet.

### Claim 29 (depends on 26)

The method for producing a steel sheet according to claim 26, wherein, after the steel sheet has been immersed in the plating bath in the coating, the steel sheet is heated to a temperature in a range of 480° C. to 600° C. in order to perform alloying.

### Claim 30 (depends on 27)

The method for producing a steel sheet according to claim 27, wherein, after the steel sheet has been immersed in the plating bath in the coating, the steel sheet is heated to a temperature in a range of 480° C. to 600° C. in order to perform alloying.

### Claim 31 (depends on 28)

The method for producing a steel sheet according to claim 28, wherein, after the steel sheet has been immersed in the plating bath in the coating, the steel sheet is heated to a temperature in a range of 480° C. to 600° C. in order to perform alloying.