# US 2019/0194774 A1 · Cold-rolled high-strength steel plate having excellent phosphating performance and formability and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0194774 A1
- Document ID: US20190194774A1
- Status: Published application
- Kind: A1
- Application number: 16/328,991
- Filed: 2017-08-29
- Published: 2019-06-27
- Earliest claimed: 2016-08-30
- Assignees: Baoshan Iron & Steel Co., Ltd.
- Applicants: Baoshan Iron & Steel Co., Ltd.
- Inventors: Shu ZHOU; Yong ZHONG; Xinyan JIN; Li WANG
- Web page: https://patentgrep.com/patent/US20190194774A1

## CPC

- C21D 9/46: for sheet metals
- C21D 1/26: Methods of annealing
- C21D 1/74: Methods of treatment in inert gas, controlled atmosphere, vacuum or pulverulent material
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/021: involving particular fabrication steps or treatments of ingots or slabs
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/28: with titanium or zirconium
- C22C 38/38: with more than 1.5% by weight of manganese
- C21D 2211/001: Austenite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- Y02P 10/20: Recycling
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A cold-rolled steel plate (1) and a manufacturing method therefor. The chemical composition of the steel plate (1) in percentage by weight is: C 0.15-0.25%, Si 1.50-2.50%, Mn 2.00-3.00%, P≤0.02%, S≤0.01%, Al 0.03-0.06%, N≤0.01%, with the balance being Fe and impurities. The surface layer has an inner oxide layer (2) with a thickness of 1-5 μm, and there is no enrichment of Si or Mn on the surface. The steel plate (1) has good phosphating performance and formability, with a tensile strength of ≥1180 MPa and an elongation of ≥14%, and has a complex-phase structure of ferrite, martensite, and retained austenite, the content of the retained austenite being not lower than 5%. A dew point is at −25° C. to 10° C. in continuous annealing, such that external oxidation transitions to internal oxidation.

## Claims

### Claim 1

A cold-rolled high-strength steel plate having excellent phosphatability and formability, comprising chemical elements in percentage by mass of: C 0.15 to 0.25%, Si 1.50 to 2.50%, Mn 2.00 to 3.00%, P≤0.02%, S≤0.01%, Al 0.03 to 0.06%, N≤0.01%, and a balance of Fe and unavoidable impurity elements, wherein a surface layer of the steel plate comprises an inner oxide layer having a thickness of 1 to 5 μm; the inner oxide layer comprises iron as a matrix; the matrix comprises oxide particles which are at least one of oxides of Si, composite oxides of Si and Mn; no Si or Mn element is enriched in the surface;
the oxide particles have an average diameter of 50 to 200 nm and an average spacing X, between the oxide particles satisfying the following relationship:
A=0.247×(0.94×[Si]+0.68×[Mn])1/2×d
B=1.382×(0.94×[Si]+0.68×[Mn])1/2×d
A≤λ≤B
wherein [Si] is the content % of Si in the steel; [Mn] is the content % of Mn in the steel; and d is the diameter of the oxide particles in nm.

### Claim 2 (depends on 1)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 1, wherein the steel plate further comprises at least one of Cr 0.01 to 1.0%, Mo 0.01 to 0.5% and Ni 0.01 to 2.0%, and/or further comprises at least one of Ti 0.005 to 0.05%, Nb 0.005 to 0.1% and V 0.005 to 0.1%.

### Claim 3

(canceled)

### Claim 4 (depends on 1)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 1, wherein the oxide particles are at least one of silicon oxide, manganese silicate, iron silicate and ferromanganese silicate.

### Claim 5 (depends on 1)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 1, wherein the cold-rolled high-strength steel plate having excellent phosphatability and formability comprises a room temperature structure having a composite structure of ferrite, martensite and residual austenite, wherein the residual austenite has a content of no less than 5%.

### Claim 6 (depends on 1)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 1, wherein the cold-rolled high-strength steel plate has a tensile strength ≥1180 MPa, and an elongation ≥14%.

### Claim 7 (depends on 1)

A manufacturing method for the cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 1, comprising the following steps:
1) Smelting and Casting
Smelting and casting according to said chemical composition to form a slab;
2) Hot Rolling and Coiling
Heating the slab to 1170-1300° C.; holding for 0.5-4 h; rolling, with a final rolling temperature ≥850° C.; and coiling at a coiling temperature of 400-700° C. to obtain a hot rolled coil;
3) Pickling and Cold Rolling
Uncoiling the hot rolled coil, pickling at a speed ≤150 m/min, and cold rolling with a cold rolling reduction of 40-80% to obtain a rolled hard strip steel;
4) Continuous Annealing
Uncoiling the resulting rolled hard strip steel, cleaning, heating to a soaking temperature of 790-920° C., and holding for 30-200 s, wherein a heating rate is 1-20° C./s, and an atmosphere of the heating and holding stages is a N2—H2 mixed gas, wherein a H2 content is 0.5-20%; wherein a dew point of an annealing atmosphere is from −25° C. to 10° C.;
then rapid cooling to 200-300° C. at a cooling rate ≥30° C./s;
then reheating to 350-450° C. and holding for 60-250 s to obtain the cold-rolled high-strength steel plate having excellent phosphatability and formability.

### Claim 8 (depends on 7)

The manufacturing method for the cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 7, wherein when the hot rolling in step 2) is performed, the temperature for reheating the slab is 1210-1270° C., and the coiling temperature is 450-550° C.

### Claim 9 (depends on 7)

The manufacturing method for the cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 7, wherein in step 4), the soaking temperature is 810-870° C., and the dew point of the annealing atmosphere is from −10° C. to 5° C.

### Claim 10 (depends on 2)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 2, wherein the oxide particles are at least one of silicon oxide, manganese silicate, iron silicate and ferromanganese silicate.

### Claim 11 (depends on 8)

The manufacturing method for the cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 8, wherein in step 4), the soaking temperature is 810-870° C., and the dew point of the annealing atmosphere is from −10° C. to 5° C.

### Claim 12 (depends on 7)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 7, wherein the steel plate further comprises at least one of Cr 0.01 to 1.0%, Mo 0.01 to 0.5% and Ni 0.01 to 2.0%, and/or further comprises at least one of Ti 0.005 to 0.05%, Nb 0.005 to 0.1% and V 0.005 to 0.1%.

### Claim 13 (depends on 7)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 7, wherein the oxide particles are at least one of silicon oxide, manganese silicate, iron silicate and ferromanganese silicate.

### Claim 14 (depends on 7)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 7, wherein the cold-rolled high-strength steel plate having excellent phosphatability and formability comprises a room temperature structure having a composite structure of ferrite, martensite and residual austenite, wherein the residual austenite has a content of no less than 5%.

### Claim 15 (depends on 7)

The cold-rolled high-strength steel plate having excellent phosphatability and formability according to claim 7, wherein the cold-rolled high-strength steel plate has a tensile strength ≥1180 MPa, and an elongation ≥14%.