# US 2019/0173091 A1 · Copper foil for current collector of lithium secondary battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0173091 A1
- Document ID: US20190173091A1
- Status: Published application
- Kind: A1
- Application number: 16/222,066
- Filed: 2018-12-17
- Published: 2019-06-06
- Earliest claimed: 2017-12-04
- Assignees: Chang Chun Petrochemical Co., Ltd.
- Applicants: Chang Chun Petrochemical Co., Ltd.
- Inventors: Huei-Fang HUANG; Kuei-Sen CHENG; Yao-Sheng LAI; Jui-Chang CHOU
- Web page: https://patentgrep.com/patent/US20190173091A1

## CPC

- H01M 4/661: {Metal or alloys, e.g. alloy coatings (H01M4/669 take precedence)}
- C25D 1/04: Wires; Strips; Foils
- C25D 3/38: of copper
- C25D 7/0614: {Strips or foils}
- C25D 7/0642: {Anodes}
- H01M 4/045: {Electrochemical coating; Electrochemical impregnation}
- H01M 4/38: of elements or alloys
- H01M 10/052: Li-accumulators
- H01M 2004/027: {Negative electrodes}
- H01M 2220/20: Batteries in motive systems, e.g. vehicle, ship, plane
- Y02E 60/10: Energy storage using batteries
- Y10T 428/12431: Foil or filament smaller than 6 mils
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

Electrodeposited copper foils having adequate puncture strength to withstand both pressure application during consolidation with negative electrode active materials during manufacture, as well as expansion/contraction during repeated charge/discharging cycles when used in a rechargeable secondary battery are described. These copper foils find specific utility as current collectors in rechargeable secondary batteries, particularly in lithium secondary battery with high capacity. Methods of making the copper foils, methods of producing negative electrode for use in lithium secondary battery and lithium secondary battery of high capacity are also described.

## Claims

### Claim at position 1

1-4. (canceled)

### Claim 5

A method of making an electrodeposited copper foil, having an area weight of the electrodeposited copper foil in the range of 26.7-329.4 g/m2, and a puncture strength Y, the puncture strength Y of the electrodeposited copper foil must lie in a range defined between a maximum value, Y1 (in N), and a minimum value, Y2 (in N), wherein the value Y1 is calculated by the following formula 1:
Y1=−0.00007*X2+0.075*X−1.3373 formula 1:
and the value Y2 is calculated by the following formula 2:
Y2=0.00003*X2+0.0247*X−0.6454 formula 2:
wherein X in each of formulas 1 and 2 represents the area weight of the electrodeposited copper foil (g/m2), and Y in each of formulas 1 and 2 represents the puncture strength of the electrodeposited copper foil (in N);
comprising electrolytically depositing the copper foil from a copper-containing electrolyte solution, wherein the electrolyte solution further comprises 200-500 ppm of nickel.

### Claim at position 3

6-7. (canceled)

### Claim 8

An electrodeposited copper foil having a drum side and a deposit side, each of the deposit side and drum side comprise a grain size, wherein the difference in grain size is less than 0.55 μm and the number of voids in the electrodeposited copper foil is less than 5 per μm2.

### Claim 9 (depends on 8)

The electrodeposited copper foil of claim 8, which copper foil has a puncture strength, wherein the puncture strength of the drum side and deposited side is at least 0.04 N.

### Claim 10 (depends on 8)

The electrodeposited copper foil of claim 8, further comprising a surface roughness (Rz) of the deposit side is less than 2.0 μm.

### Claim 11 (depends on 8)

The electrodeposited copper foil of claim 8, wherein the copper foil further comprises nickel, which nickel was electrodeposited simultaneously with the deposition of the copper foil.

### Claim 12 (depends on 9)

The electrodeposited copper foil of claim 9, wherein the area weight of the electrodeposited copper foil is in the range of 26.7-329.4 g/m2.

### Claim 13 (depends on 8)

A negative electrode comprising a consolidated electrode active material on the electrodeposited copper foil of claim 8.

### Claim 14 (depends on 13)

A rechargeable secondary battery comprising the negative electrode of claim 13.

### Claim 15 (depends on 14)

The rechargeable secondary battery of claim 14, in the form of a stack of alternating positive and negative electrodes separated by a separator, wherein at least one of the current collectors in the alternating stack comprises the negative electrode active material.

### Claim 16 (depends on 15)

An electric vehicle (EV) comprising the rechargeable secondary battery of claim 15.

### Claim 17

A method of making a negative electrode for a high capacity rechargeable secondary battery, the method comprising:
consolidating an electrode active material onto a copper foil having an area weight of the electrodeposited copper foil in the range of 26.7-329.4 g/m2, and a puncture strength Y, the puncture strength Y of the electrodeposited copper foil must lie in a range defined between a maximum value, Y1 (in N), and a minimum value, Y2 (in N), wherein the value Y1 is calculated by the following formula 1:
Y1=−0.00007*X2+0.075*X−1.3373 formula 1:
and the value Y2 is calculated by the following formula 2:
Y2=0.00003*X2+0.0247*X−0.6454 formula 2:
wherein X in each of formulas 1 and 2 represents the area weight of the electrodeposited copper foil (g/m2), and Y in each of formulas 1 and 2 represents the puncture strength of the electrodeposited copper foil (in N);
the consolidating step comprising depositing the electrode active material onto the copper foil and applying elevated pressure to both the electrode active material and the copper foil to both compress the electrode active material and to consolidate the electrode active material with the copper foil.