# US 2019/0099940 A1 · Direct writing of conformal and free-form magnets

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0099940 A1
- Document ID: US20190099940A1
- Status: Published application
- Kind: A1
- Application number: 15/722,829
- Filed: 2017-10-02
- Published: 2019-04-04
- Earliest claimed: 2017-10-02
- Assignees: United Technologies Corporation
- Applicants: United Technologies Corporation
- Inventors: Sameh Dardona; Paul Sheedy; Wayde R. Schmidt; Dustin D. Caldwell; Slade R. Culp
- Web page: https://patentgrep.com/patent/US20190099940A1

## CPC

- B29C 64/129: characterised by the energy source therefor, e.g. by global irradiation combined with a mask
- B29C 64/106: using only liquids or viscous materials, e.g. depositing a continuous bead of viscous material
- B33Y 10/00: Processes of additive manufacturing
- B33Y 70/10: Composites of different types of material, e.g. mixtures of ceramics and polymers or mixtures of metals and biomaterials
- B33Y 80/00: Products made by additive manufacturing
- H01F 1/0027: {Thick magnetic films (forming thick magnetic films H01F41/16)}
- H01F 1/44: of magnetic liquids, e.g. ferrofluids (particles in a bonding agent H01F1/28, H01F1/36, {H01F1/37})
- H01F 41/0253: {for manufacturing permanent magnets}
- H01F 41/16: the magnetic material being applied in the form of particles, e.g. by serigraphy {, to form thick magnetic films or precursors therefor} (H01F41/18 {-H01F41/24} take precedence)
- B29K 2105/16: Fillers
- B29K 2505/00: Use of metals, their alloys or their compounds, as filler
- B29K 2995/0008: Magnetic or paramagnetic
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- B33Y: ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS

## Abstract

A system for direct writing a conformal or free-form magnet includes producing a magnetic ink compound by mixing an photopolymer base and a magnetic material powder, extruding a layer of the magnetic ink compound through a nozzle on to a target substrate to form a layer, soft-curing the layer by exposing the layer to a first light, repeatedly extruding a layer and soft-curing the layer, then post-curing the magnet by exposing the magnet to a second light and an elevated temperature.

## Claims

### Claim 1

A magnetic ink compound, comprising:
a photopolymer resin base; and
a magnetic material powder.

### Claim 2 (depends on 1)

The magnetic ink compound of claim 1, wherein the photopolymer resin base is heat curable.

### Claim 3 (depends on 1)

The magnetic ink compound of claim 1, wherein the magnetic material powder comprises between 10% and 85% by volume of the magnetic ink compound.

### Claim 4 (depends on 1)

The magnetic ink compound of claim 1, wherein the magnetic material powder comprises approximately 45% by volume of the magnetic ink compound.

### Claim 5 (depends on 1)

The magnetic ink compound of claim 1, wherein the magnetic material powder is an alloy comprised of neodymium, iron, and boron.

### Claim 6 (depends on 5)

The magnetic ink compound of claim 5, wherein the magnetic material powder is comprised of particles of the alloy, wherein the particles have an average mean diameter between 1 μm and 30 μm.

### Claim 7 (depends on 1)

An additive manufacturing direct writing method of producing a magnetic pattern on a substrate comprising the magnetic ink compound of claim 1, further comprising the steps of:
(a) extruding a plurality of filaments of the magnetic ink compound through a nozzle on to the substrate, each of the filaments having a filament width and filament length, wherein there is a relative motion between the nozzle and the target substrate and wherein the filament length is at least as great as the filament width;
(b) soft-curing the first and second filaments of magnetic ink compound;
repeating steps (a) and (b) to extrude and soft-cure multiple additional filaments of magnetic ink compound above the first and second filaments of magnetic ink compound to produce the magnetic pattern; and
post-curing the magnetic pattern.

### Claim 8 (depends on 7)

The additive manufacturing direct writing method of claim 7, wherein the first filament width is between 50 μm and 500 μm.

### Claim 9 (depends on 7)

The additive manufacturing direct writing method of claim 7, wherein the soft-curing further comprises the step of exposing the layer to a first light exposure.

### Claim 10 (depends on 9)

The additive manufacturing direct writing method of claim 9, wherein the first light exposure has a wavelength between 100 nm and 425 nm.

### Claim 11 (depends on 9)

The additive manufacturing direct writing method of claim 9, wherein the first light exposure has a wavelength of approximately 365 nm.

### Claim 12 (depends on 9)

The additive manufacturing direct writing method of claim 9, wherein the first light exposure has a wavelength of approximately 405 nm.

### Claim 13 (depends on 8)

The additive manufacturing direct writing method of claim 8, wherein the post-curing further comprises the step of exposing the magnet to a second light exposure and an elevated temperature.

### Claim 14 (depends on 13)

The additive manufacturing direct writing method of claim 13, wherein the second light exposure has a wavelength between 100 nm and 425 nm.

### Claim 15 (depends on 13)

The additive manufacturing direct writing method of claim 13, wherein the second light exposure has a wavelength of approximately 365 nm.

### Claim 16 (depends on 13)

The additive manufacturing direct writing method of claim 13, wherein the second light exposure has a wavelength of approximately 405 nm.

### Claim 17 (depends on 13)

The additive manufacturing direct writing method of claim 13, wherein the elevated temperature is between 55° C. and 85° C.

### Claim 18 (depends on 13)

The additive manufacturing direct writing method of claim 13, wherein the elevated temperature is approximately 70° C.

### Claim 19

A method of producing a magnet comprising the steps of:
producing a magnetic ink compound, comprising:
a photopolymer resin base; and
a magnetic material powder; and
direct writing a magnet, further comprising the steps of:
(a) extruding a first filament having a first filament width of the magnetic ink compound through a nozzle on to a target substrate, wherein there is a relative motion between the nozzle and the target substrate;
(b) extruding a second filament having a second filament width of the magnetic ink compound through a nozzle on to a target substrate;
wherein the second filament width is approximately equal to the first filament width; and
the first filament and the at least one second filament comprise a layer;
(c) soft-curing the layer;
repeating steps (a), (b), and (c) to extrude and soft-cure multiple layers to produce the magnet; and
post-curing the magnet.

### Claim 20 (depends on 19)

The method of producing a magnet of claim 19, further comprising the step of post-curing the magnet by exposing the magnet to an elevated temperature, wherein the elevated temperature is greater than 55° C.