# US 2019/0096768 A1 · Fin isolation structures of semiconductor devices

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2019/0096768 A1
- Document ID: US20190096768A1
- Status: Published application
- Kind: A1
- Application number: 15/718,752
- Filed: 2017-09-28
- Published: 2019-03-28
- Earliest claimed: 2017-09-28
- Assignees: Taiwan Semiconductor Manufacturing Company, Ltd.
- Applicants: Taiwan Semiconductor Manufacturing Co., Ltd.
- Inventors: Kuo-Cheng Ching; Chih-Hao Wang; Kuan-Lun Cheng; Yen-Ming Chen
- Web page: https://patentgrep.com/patent/US20190096768A1

## CPC

- H10D 84/038: {using silicon technology, e.g. SiGe}
- H10D 30/0243: {using dummy structures having essentially the same shapes as the semiconductor bodies, e.g. to provide stability}
- H10D 84/0151: {Manufacturing their isolation regions}
- H10D 84/834: {comprising FinFETs}
- H10P 14/6308: {of Group IV semiconductors}
- H10W 10/012: {using local oxidation of silicon [LOCOS]}
- H10W 10/13: formed using local oxidation of silicon [LOCOS], e.g. sealed interface localised oxidation [SILO] or side-wall mask isolation [SWAMI]
- H10D 84/0158: {the components including FinFETs}
- H10D: INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10

## Abstract

A method of forming a fin field effect transistor (finFET) on a substrate includes forming a fin structure on the substrate and forming a shallow trench isolation (STI) region on the substrate. First and second fin portions of the fin structure extend above a top surface of the STI region. The method further includes oxidizing the first fin portion to convert a first material of the first fin portion to a second material. The second material is different from the first material of the first fin portion and a material of the second fin portion. The method further includes forming an oxide layer on the oxidized first fin portion and the second fin portion and forming first and second polysilicon structures on the oxide layer.

## Claims

### Claim 1

A method of forming a fin field effect transistor (finFET) on a substrate, the method comprising:
forming a fin structure on the substrate;
forming a shallow trench isolation (STI) region on the substrate, wherein first and second fin portions of the fin structure extend above a top surface of the STI region;
oxidizing the first fin portion to convert a first material of the first fin portion to a second material, wherein the second material is different from the first material of the first fin portion and a material of the second fin portion;
forming an oxide layer on the oxidized first fin portion and the second fin portion; and
forming first and second polysilicon structures on the oxide layer.

### Claim 2 (depends on 1)

The method of claim 1, wherein the oxidizing the first fin portion comprises selectively oxidizing the first fin portion without oxidizing the second fin portion.

### Claim 3 (depends on 2)

The method of claim 2, wherein the selectively oxidizing the first fin portion comprises:
forming a masking layer on the first and second fin portions;
etching a portion of the masking layer on the first fin portion to expose the first fin portion; and
oxidizing the exposed first fin portion.

### Claim 4 (depends on 2)

The method of claim 2, wherein the selectively oxidizing the first fin portion comprises:
forming a masking layer on the first and second fin portions;
forming a patterned photoresist layer on the masking layer, the patterned photoresist layer having an opening on a portion of the masking layer on the first fin portion;
etching the portion of the masking layer through the opening to expose the first fin portion; and
oxidizing the exposed first fin portion.

### Claim 5 (depends on 4)

The method of claim 4, wherein the masking layer has a thickness ranging from about 2 nm to about 4 nm.

### Claim 6 (depends on 1)

The method of claim 1, further comprising replacing the first and second polysilicon structures with respective first and second gate structures.

### Claim 7 (depends on 1)

The method of claim 1, wherein the oxidizing the first fin portion comprises exposing the first fin portion to a flow of steam at a temperature ranging from about 400° C. to about 500° C.

### Claim 8 (depends on 1)

The method of claim 1, wherein the oxidizing the first fin portion comprises:
forming a masking layer on the first and second fin portions;
etching a portion of the masking layer on the first fin portion to expose the first fin portion; and
annealing the exposed first fin portion in steam at a temperature ranging from about 400° C. to about 500° C.

### Claim 9 (depends on 1)

The method of claim 1, wherein the second material of the first fin portion comprises a doped oxide material.

### Claim 10

A method of forming a fin field effect transistor (finFET) on a substrate, the method comprising:
forming a fin structure on the substrate;
oxidizing a fin portion of the fin structure to convert a material of the fin portion to an oxide material that is different from a material of other fin portions of the fin structure;
forming an oxide layer on the oxidized fin portion and the other fin portions;
forming a polysilicon structure on the oxide layer; and
replacing the polysilicon structure with a gate structure.

### Claim 11 (depends on 10)

The method of claim 10, wherein the oxidizing the fin portion comprises:
forming a masking layer on the fin portion and the other fin portions of the fin structure;
etching a portion of the masking layer on the fin portion to expose the fin portion; and
oxidizing the exposed fin portion.

### Claim 12 (depends on 10)

The method of claim 10, wherein the oxidizing the fin portion comprises:
forming a masking layer on the fin portion and the other fin portions of the fin structure;
forming a patterned photoresist layer on the masking layer, the patterned photoresist layer having an opening on a portion of the masking layer on the fin portion;
etching the portion of the masking layer through the opening to expose the fin portion; and
oxidizing the exposed fin portion.

### Claim 13 (depends on 12)

The method of claim 12, wherein the masking layer has a thickness ranging from about 2 nm to about 4 nm.

### Claim 14 (depends on 10)

The method of claim 10, wherein the oxidizing the fin portion comprises exposing the fin portion to a flow of steam at a temperature ranging from about 400° C. to about 500° C.

### Claim 15 (depends on 10)

The method of claim 10, wherein the oxide material comprises a doped oxide material.

### Claim at position 16

16-20. (canceled)

### Claim 21

A method of forming a fin field effect transistor (finFET), the method comprising:
forming first and second fin structures on a substrate, wherein the first fin structure has a first vertical dimension;
oxidizing the second fin structure to convert a material of the second fin structure to an oxide material that is different from a material of the first fin structure, wherein the oxidized second fin structure has a second vertical dimension smaller than the first vertical dimension;
forming an oxide layer on the first fin structure and the oxidized second fin structure;
forming a polysilicon structure on the oxide layer; and
replacing the polysilicon structure with a gate structure.

### Claim 22 (depends on 21)

The method of claim 21, wherein the oxidized second fin structure comprises first and second horizontal dimensions that are different from each other.

### Claim 23 (depends on 21)

The method of claim 21, wherein the oxidizing the second fin structure comprises exposing the second fin structure to a flow of steam at a temperature ranging from about 400° C. to about 500° C.

### Claim 24 (depends on 21)

The method of claim 21, wherein the oxidizing the second fin structure comprises:
forming a masking layer on the first and second fin structures;
forming a patterned photoresist layer on the masking layer, the patterned photoresist layer comprises an opening on at least a portion of the masking layer on the second fin structure;
etching the portion of the masking layer through the opening to expose the second fin structure; and
oxidizing the exposed second fin structure.

### Claim 25 (depends on 24)

The method of claim 24, wherein the masking layer comprises a thickness ranging from about 2 nm to about 4 nm.