# US 2018/0323431 A1 · Nickel-cobalt composite hydroxide and method and device for producing same, cathode active material for non-aqueous electrolyte secondary battery and method for producing same, and non-aqueous electrolyte secondary battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2018/0323431 A1
- Document ID: US20180323431A1
- Status: Published application
- Kind: A1
- Application number: 16/028,479
- Filed: 2018-07-06
- Published: 2018-11-08
- Earliest claimed: 2012-09-28
- Assignees: Sumitomo Metal Mining Co., Ltd.
- Applicants: Sumitomo Metal Mining Co., Ltd.
- Inventors: KATSUYA KASE; YASUTAKA KAMATA; KAZUOMI RYOSHI
- Web page: https://patentgrep.com/patent/US20180323431A1

## CPC

- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- B01J 19/24: Stationary reactors without moving elements inside (B01J19/08, B01J19/26 take precedence; with stationary particles B01J8/02)
- C01G 53/42: containing alkali metals, e.g. LiNiO2
- C01G 53/66: containing alkaline earth metals, e.g. SrNiO3 or SrNiO2
- C01G 53/84: Hydroxides
- H01M 4/049: {Manufacturing of an active layer by chemical means}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- B01J 2219/00033: Continuous processes
- B01J 2219/24: Stationary reactors without moving elements inside
- C01P 2004/51: Particles with a specific particle size distribution
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2006/11: Powder tap density
- H01M 2004/028: {Positive electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

To improve cycling characteristics of a non-aqueous electrolyte secondary battery by obtaining a nickel-cobalt composite hydroxide having a sharp particle size distribution as a precursor, a slurry including a nickel-cobalt composite hydroxide obtained by continuously supplying an aqueous solution that includes at least nickel and cobalt, an ammonium ion donor aqueous solution and a caustic alkali aqueous solution to a reaction vessel and reacting, is continuously extracted and separated into a large particle size portion and s small particle size portion by classification, and the small particle size portion is continuously returned to the reaction vessel. As a result, a nickel-cobalt composite hydroxide is obtained that is expressed by the general formula: Ni1−x−yCoxMy(OH)2 (where, 0.05≤x≤0.50, 0≤y≤0.10, 0.05≤x+y≤0.50, and M is at least one kind of metal element selected from among Al, Mg, Mn, Ti, Fe, Cu, Zn and Ga, and that satisfies the relationships (D50−D10)/D50≤0.30, and (D90−D50)/D50≤0.30 among D10, D50 and D90 of this composite hydroxide.

## Claims

### Claim 1

A method for producing a nickel-cobalt composite hydroxide, the method comprising the steps of:
(a) obtaining, in a reaction process, a nickel-cobalt composite hydroxide by continuously supplying an aqueous solution including nickel and cobalt, an aqueous solution including an ammonium ion donor, and a caustic alkali aqueous solution to a reaction vessel and causing a reaction;
(b) continuously extracting, in a separation process, a slurry that includes the nickel-cobalt composite hydroxide from the reaction vessel, and separating the slurry into a large particle size portion and a small particle size portion by classification; and
(c) continuously returning, in a reflux process, the small particle size portion to the reaction vessel,
wherein the nickel-cobalt composite hydroxide comprises
a general formula of Ni1−x−yCoxMy(OH)2 (where, 0.05≤x≤0.50, 0≤y≤0.10, 0.05≤x+y≤0.50, and M is at least one kind of metal element selected from among Al, Mg, Mn, Ti, Fe, Cu, Zn and Ga,
an average particle size of within a range from 10 μm to 30 μm, and
(D50−D10)/D50≤0.30, and (D90−D50)/D50≤0.30 among D10, D50 and D90 of the nickel-cobalt composite hydroxide.

### Claim 2 (depends on 2)

The method of claim 2, wherein the nickel-cobalt composite hydroxide has a tap density of 2.0 g/cm3 or greater.

### Claim 3 (depends on 1)

The method of claim 1, wherein step (b) is performed using a wet separation apparatus that uses centrifugal force.

### Claim 4 (depends on 1)

The method of claim 1, further comprising step (d) covering a surface area of the large particle size portion separated by the separation process with an added element M, wherein M is a metal selected from among Al, Mg, Mn, Ti, Fe, Cu, Zn and Ga.

### Claim 5

A method for producing a cathode active material for a non-aqueous electrolyte secondary battery, the method comprising the steps of:
(a) forming, in a mixing process, a lithium mixture by mixing the nickel-cobalt composite hydroxide or a nickel-cobalt composite oxide,
the nickel-cobalt composite hydroxide being produced by
(i) obtaining, in a reaction process, a nickel-cobalt composite hydroxide by continuously supplying an aqueous solution including nickel and cobalt, an aqueous solution including an ammonium ion donor, and a caustic alkali aqueous solution to a reaction vessel and causing a reaction;
(ii) continuously extracting, in a separation process, a slurry that includes the nickel-cobalt composite hydroxide from the reaction vessel, and separating the slurry into a large particle size portion and a small particle size portion by classification; and
(iii) continuously returning, in a reflux process, the small particle size portion to the reaction vessel,
wherein the nickel-cobalt composite hydroxide comprises
a general formula of Ni1−x−yCoxMy(OH)2 (where, 0.05≤x≤0.50, 0≤y≤0.10, 0.05≤x+y≤0.50, and M is at least one kind of metal element selected from among Al, Mg, Mn, Ti, Fe, Cu, Zn and Ga,
an average particle size of within a range from 10 μm to 30 μm, and
(D50−D10)/D50≤0.30, and (D90−D50)/D50≤0.30 among D10, D50 and D90 of the nickel-cobalt composite hydroxide,
the nickel-cobalt composite oxide being produced by
(iv) roasting the nickel-cobalt composite hydroxide in an oxidizing atmosphere at a temperature of 300° C. to 700° C., and a lithium compound; and
(v) performing calcination, in a calcination process, of the lithium mixture in an oxidizing atmosphere at a temperature of 600° C. to 850° C.