# US 2018/0320262 A1 · Carbo-nitriding process for martensitic stainless steel and stainless steel article having improved corrosion resistance

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2018/0320262 A1
- Document ID: US20180320262A1
- Status: Published application
- Kind: A1
- Application number: 16/039,564
- Filed: 2018-07-19
- Published: 2018-11-08
- Earliest claimed: 2011-06-02
- Assignees: UES, Inc.; Midwest Thermal-Vac Inc.; Aktiebolaget Skf
- Applicants: Ues Inc.; Midwest Thermal-Vac Inc; Aktiebolaget Skf
- Inventors: Hitesh K. Trivedi; Frederick J. Otto; Timothy W. Piazza; Bryan A. McCoy; Rabi S. Bhattacharya
- Web page: https://patentgrep.com/patent/US20180320262A1

## CPC

- C23C 8/32: of ferrous surfaces
- C21D 1/06: Surface hardening
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 6/005: {containing Mn}
- C21D 6/007: {containing Co}
- C21D 9/40: for rings; for bearing races
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/52: with cobalt
- C23C 8/58: more than one element being applied in more than one step
- F16C 33/62: Selection of substances
- F16C 33/64: Special methods of manufacture
- C21D 2211/008: Martensite
- C22C 5/04: Alloys based on a platinum group metal
- C22C 19/03: based on nickel
- F16C 2202/04: Hardness
- F16C 2204/70: with chromium as the next major constituent
- F16C 2240/06: Temperature
- F16C 2240/60: Thickness, e.g. thickness of coatings
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F16C: SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS

## Abstract

A method for producing a case-hardened martensitic stainless steel article includes: providing an article comprised, at least in part, of a martensitic stainless steel, carburizing the article within a temperature range of 1625° F.-1680° F. (885° C.-916° C.), and then carbo-nitriding the article within a temperature range of 1575° F.-1625° F. (857° C.-885° C.). An article, such as a bearing ring, comprising such a case-hardened martensitic stainless steel is also disclosed.

## Claims

### Claim 1

A method comprising:
(a) providing an article comprised, at least in part, of a martensitic stainless steel,
(b) carburizing the article within a temperature range of 1625° F.-1680° F., and
(c) then carbo-nitriding the article within a temperature range of 1575° F.-1625° F., wherein carbon and nitrogen are simultaneously introduced into the case of the stainless steel, thereby producing a case-hardened martensitic stainless steel article.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the stainless steel in step (a) consists essentially of 0.02-0.50 wt % C, 0.1-1.5 wt % Mn, 0.10-2.0 wt % Si, 8.0-20.0 wt % Cr, 1.0-3.5 wt % Ni, 0.40-3.0 wt % Mo, 0.40-2.0 wt % V, 1.0-10.0 wt % Co, the balance being Fe.

### Claim 3 (depends on 2)

The method according to claim 2, wherein stainless steel in step (a) consists essentially of 0.03-0.10 wt % C, 0.5-1.0 wt % Mn, 0.20-0.6 wt % Si, 11.0-15.0 wt % Cr, 2.40-3.0 wt % Ni, 1.50-2.0 wt % Mo, 0.40-0.80 wt % V, 5.0-6.0 wt % Co, the balance being Fe.

### Claim 4 (depends on 2)

The method according to claim 2, wherein the stainless steel in step (a) contains the following weight percentages of elements:
Mo+V=0.8 to 4.0 wt % and
Co+Ni=2.0 to 12.0 wt %.

### Claim 5

(canceled)

### Claim 6 (depends on 1)

The method according to claim 1, wherein a nitrogen:carbon differential ratio in step (c) is between about 6-8:1.

### Claim 7 (depends on 6)

The method according to claim 6, wherein nitrogen is provided by ammonia and carbon is provided by acetylene and/or propane.

### Claim 8 (depends on 1)

The method according to claim 1, wherein the total time for steps (b) and (c) is between 15-18 hours.

### Claim at position 9

-11. (canceled)

### Claim 12 (depends on 1)

The method according to claim 1, wherein step (c) is performed until the case-hardened martensitic stainless steel article contains carbon in the range of 1.5-2 wt % in the hardened case at least up to a depth of 500 μm.

### Claim 13 (depends on 1)

The method according to claim 1, wherein the case-hardened martensitic stainless steel article is subsequently:
(d) quenched in liquid nitrogen and
(e) then tempered twice at about 575° F.-625° F. (301° C.-329° C.) for 2 hours.

### Claim at position 12

-21. (canceled)

### Claim 22 (depends on 1)

The method according to claim 1, wherein the article is a bearing ring.

### Claim at position 14

-25. (canceled)

### Claim 26 (depends on 4)

The method according to claim 4, wherein a nitrogen:carbon differential ratio in step (c) is between about 6-8:1.

### Claim 27 (depends on 26)

The method according to claim 26, wherein nitrogen is provided by ammonia and carbon is provided by acetylene.

### Claim 28 (depends on 27)

The method according to claim 27, wherein the total time for steps (b) and (c) is between 15-18 hours.

### Claim at position 18

-30. (canceled)

### Claim 31 (depends on 28)

The method according to claim 28, wherein the article is a bearing ring and step (c) is performed until the bearing ring contains at least 0.5 wt % nitrogen in at least one portion of the hardened case and at least 0.2 wt % nitrogen at a depth of about 200 μm.

### Claim 32 (depends on 31)

The method according to claim 31, wherein step (c) is performed until the bearing ring contains carbon in the range of 1.5-2 wt % in the hardened case at least up to a depth of 500 μm.

### Claim at position 21

-36. (canceled)

### Claim 37 (depends on 32)

The method according to claim 32, wherein the bearing ring exhibits a residual stress of at least 500 MPa in the hardened case after step (c) is completed.

### Claim 38 (depends on 37)

The method according to claim 37, wherein at least one portion of the hardened case of the bearing ring comprises at least 16 volume percent of retained austenite.

### Claim 39

(canceled)

### Claim 40

A bearing ring comprised of a carbo-nitrided martensitic stainless steel having:
a hard carburized case up to a depth of about 900-1125 μm,
a presence of nitrogen or nitrides up to depth of 250 μm,
0.3-0.7 wt % nitrogen at the surface and 0.1-0.3 wt % nitrogen at a depth of about 250 μm, and
carbon in the range of 1.5-2 wt % in the hardened case,
wherein the bearing ring has a core consisting essentially of:
0.02-0.50 wt % C, 0.1-1.5 wt % Mn, 0.10-2.0 wt % Si, 12.0-20.0 wt % Cr, 1.0-3.5 wt % Ni, 0.40-3.0 wt % Mo, 0.40-2.0 wt % V, and 1.0-10.0 wt % Co, the balance being Fe and unavoidable impurities, and the core of the bearing ring contains the following weight percentages of elements:
Mo+V=0.8 to 4.0 wt % and
Co+Ni=2.0 to 12.0 wt %.

### Claim at position 26

-52. (canceled)

### Claim 53

A method comprising:
(a) placing an article into a vacuum chamber, the article being comprised of a martensitic stainless steel consisting essentially of 0.02-0.50 wt % C, 0.1-1.5 wt % Mn, 0.10-2.0 wt % Si, 8.0-20.0 wt % Cr, 1.0-3.5 wt % Ni, 0.40-3.0 wt % Mo, 0.40-2.0 wt % V, 1.0-10.0 wt % Co, the balance being Fe,
(b) vacuum carburizing the article within a temperature range of 1625° F.-1680° F. by repeating a plurality of cycles comprising (i) introducing acetylene into the vacuum chamber and (ii) then evacuating the vacuum chamber to about 0.1 atm, and
(c) then vacuum carbo-nitriding the article within a temperature range of 1575° F.-1625° F. by repeating a plurality of cycles comprising (i) introducing acetylene and ammonia into the vacuum chamber and (ii) then evacuating the vacuum chamber to about 0.1 atm.