# US 2018/0023161 A1 · High-strength steel sheet and production method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2018/0023161 A1
- Document ID: US20180023161A1
- Status: Published application
- Kind: A1
- Application number: 15/547,659
- Filed: 2016-01-27
- Published: 2018-01-25
- Earliest claimed: 2015-02-03
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Hidekazu MINAMI; Shinjiro KANEKO; Takeshi YOKOTA; Kazuhiro SETO
- Web page: https://patentgrep.com/patent/US20180023161A1

## CPC

- C21D 9/46: for sheet metals
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A steel sheet has a microstructure that contains ferrite in an area ratio of 20% or more, martensite in an area ratio of 5% or more, and tempered martensite in an area ratio of 5% or more. The ferrite has a mean grain size of 20.0 μm or less. An inverse intensity ratio of γ-fiber to α-fiber in the ferrite is 1.00 or more and an inverse intensity ratio of γ-fiber to α-fiber in the martensite and the tempered martensite is 1.00 or more.

## Claims

### Claim 1

A high-strength steel sheet comprising:
a chemical composition that contains, by mass %, C: 0.060% or more and 0.200% or less, Si: 0.50% or more and 2.20% or less, Mn: 1.00% or more and 3.00% or less, P: 0.100% or less , S: 0.0100% or less, Al: 0.010% or more and 2.500% or less, N: 0.0100% or less, either or both Ti: 0.001% or more and 0.200% or less and Nb: 0.001% or more and 0.200% or less, and the balance consisting of Fe and incidental impurities, the chemical composition satisfying a relation of 500≦C*≦1300, where C* is determined by formula (1) or (2) given below; and
a microstructure that contains ferrite in an area ratio of 20% or more, martensite in an area ratio of 5% or more, and tempered martensite in an area ratio of 5% or more, the ferrite having a mean grain size of 20.0 μm or less, and an inverse intensity ratio of γ-fiber to α-fiber in the ferrite being 1.00 or more and an inverse intensity ratio of γ-fiber to α-fiber in the martensite and the tempered martensite being 1.00 or more:
in the case of the chemical composition containing only Ti from among Ti and Nb, or both Ti and Nb,
C*=(C−(12.0/47.9)×(Ti−(47.9/14.0)×N−(47.9/32.1)×S)−(12.0/92.9)×Nb)×10000 (1), or
in the case of the chemical composition containing only Nb from among Ti and Nb,
C*=(C−(12.0/92.9)×Nb)×10000 (2),
where each of the element symbols C, N, S, Ti, and Nb indicates content by mass % of the corresponding element in the steel sheet, and the unit of C* is mass ppm.

### Claim at position 2

2-13. (canceled)

### Claim 14

A high-strength steel sheet comprising:
a chemical composition that contains, by mass %, C: 0.060% or more and 0.200% or less, Si: 0.50% or more and 2.20% or less, Mn: 1.00% or more and 3.00% or less, P: 0.100% or less, S: 0.0100% or less, Al: 0.010% or more and 2.500% or less, N: 0.0100% or less, either or both Ti: 0.001% or more and 0.200% or less and Nb: 0.001% or more and 0.200% or less, and
at least one selected from groups (a) to (e):
(a) at least one selected from Cr: 0.05% or more and 1.00% or less, Mo: 0.05% or more and 1.00% or less, Ni: 0.05% or more and 1.00% or less, and Cu: 0.05% or more and 1.00% or less;
(b) B: 0.0003% or more and 0.0050% or less;
(c) at least one selected from Ca: 0.0010% or more and 0.0050% or less, Mg: 0.0005% or more and 0.0100% or less, and REM: 0.0003% or more and 0.0050% or less;
(d) at least one selected from Sn: 0.0020% or more and 0.2000% or less and Sb: 0.0020% or more and 0.2000% or less; and
(e) Ta: 0.0010% or more and 0.1000% or less; and
the balance consisting of Fe and incidental impurities, the chemical composition satisfying a relation of 500≦C*≦1300, where C* is determined by any one of formula (1) to (4) given below; and
a microstructure that contains ferrite in an area ratio of 20% or more, martensite in an area ratio of 5% or more, and tempered martensite in an area ratio of 5% or more, the ferrite having a mean grain size of 20.0 μm or less, and an inverse intensity ratio of γ-fiber to α-fiber in the ferrite being 1.00 or more and an inverse intensity ratio of γ-fiber to α-fiber in the martensite and the tempered martensite being 1.00 or more:
in the case of the chemical composition containing only Ti from among Ti and Nb, or both Ti and Nb, and not containing Ta,
C*=(C−(12.0/47.9)×(Ti−(47.9/14.0)×N−(47.9/32.1)×S)−(12.0/92.9)×Nb)×10000 (1),
in the case of the chemical composition containing only Nb from among Ti and Nb and, not containing Ta,
C*=(C−(12.0/92.9)×Nb)×10000 (2),
in the case of the chemical composition containing only Ti from among Ti and Nb, or both Ti and Nb, and containing Ta,
C*=(C−(12.0/47.9)×(Ti−(47.9/14.0)×N−(47.9/32.1)×S)−(12.0/92.9)×Nb−(12.0/180.9)×Ta)×10000 (3), or
in the case of the chemical composition containing only Nb from among Ti and Nb, and containing Ta,
C*=(C−(12.0/92.9)×Nb−(12.0/180.9)×Ta)×10000 (4),
where each of the element symbols C, N, S, Ti, Nb, and Ta indicates content by mass % of the corresponding element in the steel sheet, and the unit of C* is mass ppm.

### Claim 15 (depends on 1)

The high-strength steel sheet according to claim 1, wherein the high-strength steel sheet is a cold-rolled steel sheet.

### Claim 16 (depends on 14)

The high-strength steel sheet according to claim 14, wherein the high-strength steel sheet is a cold-rolled steel sheet.

### Claim 17 (depends on 1)

The high-strength steel sheet according to claim 1, wherein the high-strength steel sheet comprises a coating or plating on a surface thereof.

### Claim 18 (depends on 14)

The high-strength steel sheet according to claim 14, wherein the high-strength steel sheet comprises a coating or plating on a surface thereof.

### Claim 19 (depends on 17)

The high-strength steel sheet according to claim 17, wherein the coating or plating is a galvanized coating or plating.

### Claim 20 (depends on 18)

The high-strength steel sheet according to claim 18, wherein the coating or plating is a galvanized coating or plating.

### Claim 21 (depends on 1)

A method for producing the high-strength steel sheet according to claim 1, the method comprising:
heating a steel slab comprising the chemical composition as recited in claim 1 to a temperature range of 1150° C. to 1300° C.;
subjecting the steel slab to hot rolling with a finisher delivery temperature from 850° C. to 1000° C. to obtain a hot-rolled steel sheet;
subjecting the hot-rolled steel sheet to coiling in a temperature range of 500° C. to 800° C.;
subjecting the hot-rolled steel sheet to cold rolling at a cold rolling reduction of 40% or more to obtain a cold-rolled steel sheet;
subjecting the cold-rolled steel sheet to first heat treatment, whereby the cold-rolled steel sheet is heated to a temperature range of 450° C. to 750° C. and retained for 300 s or more in the temperature range of 450° C. to 750° C.;
then subjecting the cold-rolled steel sheet to second heat treatment, whereby the cold-rolled steel sheet is heated to a temperature of 750° C. or higher and 950° C. or lower, and subsequently cooled to a cooling stop temperature of 50° C. or higher and 250° C. or lower with a mean cooling rate of 10° C./s or higher at least in a temperature range down to 500° C.; and
then subjecting the cold-rolled steel sheet to third heat treatment, whereby the cold-rolled steel sheet is heated to a temperature range of above 250° C. to 600° C. and retained for 10 s or more in the temperature range of above 250° C. to 600° C.

### Claim 22 (depends on 21)

The method according to claim 21, further comprising:
after the third heat treatment, subjecting the cold-rolled steel sheet to coating or plating treatment.

### Claim 23 (depends on 22)

The method according to claim 22, wherein the coating or plating treatment is hot-dip galvanizing treatment.

### Claim 24 (depends on 22)

The method according to claim 22, wherein the coating or plating treatment is hot-dip galvanizing treatment to form a hot-dip galvanized coating, and the method further comprises after the hot-dip galvanizing treatment, performing alloying treatment on the hot-dip galvanized coating in a temperature range of 470° C. to 600° C.

### Claim 25 (depends on 14)

A method for producing the high-strength steel sheet according to claim 14, the method comprising:
heating a steel slab comprising the chemical composition as recited in claim 14 to a temperature range of 1150° C. to 1300° C.;
subjecting the steel slab to hot rolling with a finisher delivery temperature from 850° C. to 1000° C. to obtain a hot-rolled steel sheet;
subjecting the hot-rolled steel sheet to coiling in a temperature range of 500° C. to 800° C.;
subjecting the hot-rolled steel sheet to cold rolling at a cold rolling reduction of 40% or more to obtain a cold-rolled steel sheet;
subjecting the cold-rolled steel sheet to first heat treatment, whereby the cold-rolled steel sheet is heated to a temperature range of 450° C. to 750° C. and retained for 300 s or more in the temperature range of 450° C. to 750° C.;
then subjecting the cold-rolled steel sheet to second heat treatment, whereby the cold-rolled steel sheet is heated to a temperature of 750° C. or higher and 950° C. or lower, and subsequently cooled to a cooling stop temperature of 50° C. or higher and 250° C. or lower with a mean cooling rate of 10° C./s or higher at least in a temperature range down to 500° C.; and
then subjecting the cold-rolled steel sheet to third heat treatment, whereby the cold-rolled steel sheet is heated to a temperature range of above 250° C. to 600° C. and retained for 10 s or more in the temperature range of above 250° C. to 600° C.

### Claim 26 (depends on 25)

The method according to claim 25, further comprising:
after the third heat treatment, subjecting the cold-rolled steel sheet to coating or plating treatment.

### Claim 27 (depends on 26)

The method according to claim 26, wherein the coating or plating treatment is hot-dip galvanizing treatment.

### Claim 28 (depends on 26)

The method according to claim 26, wherein the coating or plating treatment is hot-dip galvanizing treatment to form a hot-dip galvanized coating, and the method further comprises after the hot-dip galvanizing treatment, performing alloying treatment on the hot-dip galvanized coating in a temperature range of 470° C. to 600° C.