# US 2018/0023155 A1 · Cold-rolled steel sheet and method of manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2018/0023155 A1
- Document ID: US20180023155A1
- Status: Published application
- Kind: A1
- Application number: 15/549,468
- Filed: 2016-02-24
- Published: 2018-01-25
- Earliest claimed: 2015-02-24
- Assignees: Nippon Steel & Sumitomo Metal Corporation
- Applicants: Nippon Steel & Sumitomo Metal Corporation
- Inventors: Kengo TAKEDA; Kunio HAYASHI; Akihiro UENISHI; Masafumi AZUMA; Takayuki NOZAKI; Yuri TODA
- Web page: https://patentgrep.com/patent/US20180023155A1

## CPC

- C21D 8/1233: {Cold rolling}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0436: {Cold rolling}
- C21D 9/46: for sheet metals
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/18: containing chromium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

In a cold-rolled steel sheet having a predetermined chemical composition, a metallographic structure contains 40.0% or more and less than 60.0% of a polygonal ferrite, 30.0% or more of a bainitic ferrite, 10.0% to 25.0% of a residual austenite, and 15.0% or less of a martensite, by an area ratio, in the residual austenite, a proportion of the residual austenite in which an aspect ratio is 2.0 or less, a length of a long axis is 1.0 μm or less, and a length of a short axis is 1.0 μm or less, is 80.0% or more, in the bainitic ferrite, a proportion of the bainitic ferrite in which an aspect ratio is 1.7 or less and an average value of a crystal orientation difference in a region surrounded by a boundary in which a crystal orientation difference is 15° or more is 0.5° or more and less than 3.0°, is 80.0% or more, and a connection index D value of the martensite, the bainitic ferrite, and the residual austenite is 0.70 or less.

## Claims

### Claim 1

A cold-rolled steel sheet, comprising, as a chemical composition, in % by mass:
C: 0.100% or more and less than 0.500%;
Si: 0.8% or more and less than 4.0%;
Mn: 1.0% or more and less than 4.0%;
P: less than 0.015%;
S: less than 0.0500%;
N: less than 0.0100%;
Al: less than 2.000%;
Ti: 0.020% or more and less than 0.150%;
Nb: 0% or more and less than 0.200%;
V: 0% or more and less than 0.500%;
B: 0% or more and less than 0.0030%;
Mo: 0% or more and less than 0.500%;
Cr: 0% or more and less than 2.000%;
Mg: 0% or more and less than 0.0400%;
Rem: 0% or more and less than 0.0400%;
Ca: 0% or more and less than 0.0400%; and
a remainder of Fe and impurities,
wherein the total amount of Si and Al is 1.000% or more,
wherein a metallographic structure contains 40.0% or more and less than 60.0% of a polygonal ferrite, 30.0% or more of a bainitic ferrite, 10.0% to 25.0% of a residual austenite, and 15.0% or less of a martensite, by an area ratio,
wherein, in the residual austenite, a proportion of the residual austenite in which an aspect ratio is 2.0 or less, a length of a long axis is 1.0 μm or less, and a length of a short axis is 1.0 μm or less, is 80.0% or more,
wherein, in the bainitic ferrite, a proportion of the bainitic ferrite in which an aspect ratio is 1.7 or less and an average value of a crystal orientation difference in a region surrounded by a boundary in which a crystal orientation difference is 15° or more is 0.5° or more and less than 3.0°, is 80.0% or more,
wherein a connection index D value of the martensite, the bainitic ferrite, and the residual austenite is 0.70 or less, and
wherein a tensile strength is 980 MPa or more, a 0.2% proof stress is 600 MPa or more, a total elongation is 21.0% or more, and a hole expansion ratio is 30.0% or more.

### Claim 2 (depends on 1)

The cold-rolled steel sheet according to claim 1,
wherein the connection index D value is 0.50 or less and the hole expansion ratio is 50.0% or more.

### Claim 3 (depends on 1, 2)

The cold-rolled steel sheet according to claim 1 or 2, comprising, as the chemical composition, in % by mass:
one or two or more of
Nb: 0.005% or more and less than 0.200%;
V: 0.010% or more and less than 0.500%;
B: 0.0001% or more and less than 0.0030%;
Mo: 0.010% or more and less than 0.500%;
Cr: 0.010% or more and less than 2.000%;
Mg: 0.0005% or more and less than 0.0400%;
Rem: 0.0005% or more and less than 0.0400%; and
Ca: 0.0005% or more and less than 0.0400%.

### Claim 4 (depends on 1, 2)

A hot-rolled steel sheet which is used for manufacturing the cold-rolled steel sheet according to claim 1 or 2, comprising, as a chemical composition, in % by mass:
C: 0.100% or more and less than 0.500%;
Si: 0.8% or more and less than 4.0%;
Mn: 1.0% or more and less than 4.0%;
P: less than 0.015%;
S: less than 0.0500%;
N: less than 0.0100%;
Al: less than 2.000%;
Ti: 0.020% or more and less than 0.150%;
Nb: 0% or more and less than 0.200%;
V: 0% or more and less than 0.500%;
B: 0% or more and less than 0.0030%;
Mo: 0% or more and less than 0.500%;
Cr: 0% or more and less than 2.000%;
Mg: 0% or more and less than 0.0400%;
Rem: 0% or more and less than 0.0400%;
Ca: 0% or more and less than 0.0400%; and
a remainder of Fe and impurities,
wherein the total amount of Si and Al is 1.000% or more,
wherein a metallographic structure contains a bainitic ferrite,
wherein, in the bainitic ferrite, an area ratio of the bainitic ferrite in which an average value of a crystal orientation difference in a region surrounded by a boundary in which a crystal orientation difference is 15° or more is 0.5° or more and less than 3.0°, is 80.0% or more, and
wherein a connection index E value of pearlite is 0.40 or less.

### Claim 5

A method of manufacturing a cold-rolled steel sheet, the method comprising:
casting a steel ingot or a slab including, as a chemical composition, C: 0.100% or more and less than 0.500%, Si: 0.8% or more and less than 4.0%, Mn: 1.0% or more and less than 4.0%, P: less than 0.015%, S: less than 0.0500%, N: less than 0.0100%, Al: less than 2.000%, Ti: 0.020% or more and less than 0.150%, Nb: 0% or more and less than 0.200%, V: 0% or more and less than 0.500%, B: 0% or more and less than 0.0030%, Mo: 0% or more and less than 0.500%, Cr: 0% or more and less than 2.000%, Mg: 0% or more and less than 0.0400%, Rem: 0% or more and less than 0.0400%, Ca: 0% or more and less than 0.0400%, and a remainder of Fe and impurities, in which the total amount of Si and Al is 1.000% or more;
hot rolling including a rough rolling in which the steel ingot or the slab is reduced at 40% or more in total in a first temperature range of 1000° C. to 1150° C., and a finish rolling in which the steel ingot or the slab is reduced at 50% or more in total in a second temperature range of T1° C. to T1+150° C., and the hot rolling being finished at T1−40° C. or more to obtain a hot-rolled steel sheet when a temperature determined by compositions specified in the following Equation (1) is set to be T1;
first cooling of cooling the hot-rolled steel sheet after the hot rolling at a cooling rate of 20° C./s to 80° C./s to a third temperature range of 600° C. to 650° C.;
holding the hot-rolled steel sheet after the first cooling for time t seconds to 10.0 seconds determined by the following Equation (2) in the third temperature range of 600° C. to 650° C.;
second cooling of cooling the hot-rolled steel sheet after the holding, to 600° C. or less;
coiling the hot-rolled steel sheet at 600° C. or less so that in a microstructure of the hot-rolled steel sheet after coiling, the connection index E value of the pearlite is 0.40 or less, and in the bainitic ferrite, an area ratio of the bainitic ferrite in which an average value of a crystal orientation difference in a region surrounded by a boundary in which a crystal orientation difference is 15° or more is 0.5° or more and less than 3.0°, is 80.0% or more to obtain the hot-rolled steel sheet;
pickling the hot-rolled steel sheet;
cold rolling the hot-rolled steel sheet after the pickling so that a cumulative rolling reduction is 40.0% to 80.0% to obtain a cold-rolled steel sheet;
annealing of holding the cold-rolled steel sheet after the cold rolling for 30 to 600 seconds in a fourth temperature range after raising the temperature to the fourth temperature range of T1−50° C. to 960° C.;
third cooling of cooling the cold-rolled steel sheet after the annealing at a cooling rate of 1.0° C./s to 10.0° C./s to a fifth temperature range of 600° C. to 720° C.; and
heat treating of holding the cold-rolled steel sheet for 30 seconds to 600 seconds after cooling the temperature to a sixth temperature range of 150° C. to 500° C. at the cooling rate of 10.0° C./s to 60.0° C./s,
T1(° C.)=920+40×C2−80×C+Si2+0.5×Si+0.4×Mn2−9×Mn+10×Al+200×N2−30×N−15×Ti Equation (1)
t(seconds)=1.6+(10×C+Mn−20×Ti)/8 Equation (2)
here, element symbols in the equations indicate the amount of elements in % by mass.

### Claim 6 (depends on 5)

The method of manufacturing a cold-rolled steel sheet according to claim 5,
wherein the steel sheet is coiled at 100° C. or less in the coiling.

### Claim 7 (depends on 6)

The method of manufacturing a cold-rolled steel sheet according to claim 6, comprising:
holding the hot-rolled steel sheet for 10 seconds to 10 hours after raising the temperature to a seventh temperature range of 400° C. to an Al transformation point between the coiling and the pickling.

### Claim 8 (depends on 5, 6, 7)

The method of manufacturing a cold-rolled steel sheet according to any one of claims 5 to 7, comprising:
reheating the cold-rolled steel sheet to a temperature range of 150° C. to 500° C. before holding the cold-rolled steel sheet for 1 second or more after cooling the cold-rolled steel sheet to the sixth temperature range in the heat treating.

### Claim 9 (depends on 5, 6, 7)

The method of manufacturing a cold-rolled steel sheet according to any one of claims 5 to 7, further comprising:
hot-dip galvanizing the cold-rolled steel sheet after the heat treating.

### Claim 10 (depends on 9)

The method of manufacturing a cold-rolled steel sheet according to claim 9, further comprising:
alloying of performing the heat treatment within an eighth temperature range of 450° C. to 600° C. after the hot-dip galvanizing.

### Claim 11 (depends on 8)

The method of manufacturing a cold-rolled steel sheet according to claim 8, further comprising:
hot-dip galvanizing the cold-rolled steel sheet after the heat treating.