# US 2018/0023153 A1 · Shot peening treatment for cavitation erosion resistance

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2018/0023153 A1
- Document ID: US20180023153A1
- Status: Published application
- Kind: A1
- Application number: 15/214,595
- Filed: 2016-07-20
- Published: 2018-01-25
- Earliest claimed: 2016-07-20
- Assignees: Hitachi, Ltd.
- Applicants: Hitachi, Ltd.
- Inventors: Lili ZHENG; Wei YUAN
- Web page: https://patentgrep.com/patent/US20180023153A1

## CPC

- C21D 7/06: by shot-peening or the like
- B23P 25/00: Auxiliary treatment of workpieces, before or during machining operations, to facilitate the action of the tool or the attainment of a desired final condition of the work, e.g. relief of internal stress
- B24B 39/006: {Peening and tools therefor}
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/40: with nickel
- C22C 38/44: with molybdenum or tungsten
- C22C 38/58: with more than 1.5% by weight of manganese
- B24C 1/10: for compacting surfaces, e.g. shot-peening (for deforming sheet metal, tubes or profiles B21D31/06; as a metallurgical treatment C21D7/00, C22F1/00)
- C21D 11/00: Process control or regulation for heat treatments
- C21D 2211/001: Austenite
- Y10T 29/479: by shot peening or blasting
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B23P: METAL-WORKING NOT OTHERWISE PROVIDED FOR; COMBINED OPERATIONS; UNIVERSAL MACHINE TOOLS (arrangements for copying or controlling B23Q)
- B24B: MACHINES, DEVICES, OR PROCESSES FOR GRINDING OR POLISHING (grinding of gear teeth B23F, of screw-threads B23G1/36; by electro-erosion B23H; abrasive or related blasting B24C; tools for grinding, buffing or sharpening B24D; polishing compositions C09G1/00; abrasives C09K3/14; electrolytic etching or polishing C25F3/00; grinding arrangements for use on assembled railway tracks E01B31/17); DRESSING OR CONDITIONING OF ABRADING SURFACES; FEEDING OF GRINDING, POLISHING, OR LAPPING AGENTS
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B24C: ABRASIVE OR RELATED BLASTING WITH PARTICULATE MATERIAL
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

In some examples, a material may be subject to shot peening of a relatively long duration to improve cavitation erosion resistance of the material. For example, the material surface may be shot peened to cause grain reduction and an increase in hardness to a depth of 60 μm or more, while the surface remains relatively smooth. As one example, the method may include treating a surface of austenitic stainless steel by impacting the surface with shot media for a treatment duration of 15 to 40 minutes at a shot peening intensity corresponding to an Almen strip type A intensity of 5A to 10A.

## Claims

### Claim 1

A method of treating a surface of austenitic stainless steel to increase resistance to cavitation erosion, the method comprising impacting the surface with shot media for a shot peening duration of 15 to 40 minutes at a shot peening intensity corresponding to an Almen strip type A intensity of 5A to 10A.

### Claim 2 (depends on 1)

The method as recited in claim 1, wherein the shot media is cast steel shot having a size range between 0.18 mm to 1.68 mm.

### Claim 3 (depends on 1)

The method as recited in claim 1, wherein the shot peening duration is between 20 and 30 minutes.

### Claim 4 (depends on 3)

The method as recited in claim 3, wherein the shot peening intensity is in a range from 5A to 7A, and the shot media is steel shot having a size range from 0.58 mm to 0.99 mm.

### Claim 5 (depends on 1)

The method as recited in claim 1, further comprising polishing the surface to remove 10 to 30 μm of material.

### Claim 6 (depends on 1)

The method as recited in claim 1, wherein the austenitic stainless steel includes 18-20% Cr and 2.0-3.0% Mo.

### Claim 7 (depends on 1)

The method as recited in claim 1, wherein the treatment provides in an increase in hardness to a depth of at least 60 μm from the surface and a surface roughness of less than 20 μm.

### Claim 8

A method comprising shot peening a surface of a material for a shot peening duration of 15 to 40 minutes at a shot peening intensity corresponding to an Almen strip type A intensity of 5A to 10A, wherein:
the material has an austenitic crystalline structure, and
a shot media used during the shot peening has a hardness greater than the material when the material is in an annealed condition.

### Claim 9 (depends on 8)

The method as recited in claim 8, wherein the shot media is cast steel shot having a size range between 0.18 mm to 1.68 mm.

### Claim 10 (depends on 8)

The method as recited in claim 8, wherein the shot peening duration is between 20 and 30 minutes.

### Claim 11 (depends on 8)

The method as recited in claim 8, wherein the shot peening intensity is in a range from 5A to 7A, and the shot media is steel shot having a size range from 0.58 mm to 0.99 mm.

### Claim 12 (depends on 8)

The method as recited in claim 8, further comprising:
following the shot peening, determining that a roughness of the surface exceeds 20 μm; and
decreasing at least one of:
a shot media size, or
the shot peening intensity while maintaining the shot peening intensity within a range of 5A-10A.

### Claim 13 (depends on 8)

The method as recited in claim 8, further comprising:
following the shot peening, determining that a depth of an increased hardness layer is less than 60 μm; and
increasing at least one of:
the shot peening intensity while maintaining the shot peening intensity within a range of 5A-10A, or
the shot peening duration, while maintaining the duration within a range of 15-40 minutes.

### Claim 14 (depends on 8)

The method as recited in claim 8, wherein the material is an austenitic stainless steel including 18-20% Cr and 2.0-3.0% Mo.

### Claim 15

A method comprising:
impacting a surface of a material having an austenitic crystalline structure with shot media for a duration ranging from 15 and 40 minutes at an Almen strip type A intensity ranging from 5A to 10A; and
polishing the surface to remove 10 to 20 μm of the material.

### Claim 16 (depends on 15)

The method as recited in claim 15, wherein the shot media is cast steel shot having a size range between 0.18 mm to 1.68 mm.

### Claim 17 (depends on 15)

The method as recited in claim 15, wherein the duration ranges between 20 and 30 minutes.

### Claim 18 (depends on 17)

The method as recited in claim 17, wherein the shot peening intensity is in a range from 5A to 7A, and the shot media is steel shot having a size range from 0.58 mm to 0.99 mm.

### Claim 19 (depends on 15)

The method as recited in claim 15, wherein the material is austenitic stainless steel including 18-20% Cr and 2.0-3.0% Mo.

### Claim 20 (depends on 15)

The method as recited in claim 15, wherein
following the shot peening, prior to the polishing, determining that a roughness of the surface exceeds 20 μm; and
decreasing at least one of:
a shot media size, or
the shot peening intensity while maintaining the shot peening intensity within a range of 5A-10A.