# US 2017/0362729 A1 · Fe-P-Cr ALLOY THIN PLATE AND METHOD FOR MANUFACTURING SAME

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0362729 A1
- Document ID: US20170362729A1
- Status: Published application
- Kind: A1
- Application number: 15/539,624
- Filed: 2015-12-02
- Published: 2017-12-21
- Earliest claimed: 2014-12-24
- Assignees: Posco
- Applicants: Posco
- Inventors: Dongkyun KIM; Hongseok YANG
- Web page: https://patentgrep.com/patent/US20170362729A1

## CPC

- C25D 1/20: Separation of the formed objects from the electrodes {with no destruction of said electrodes}
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/18: containing chromium
- C22C 38/40: with nickel
- C25D 1/04: Wires; Strips; Foils
- C25D 3/56: of alloys
- C22C 2200/02: Amorphous
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

The present invention relates to an Fe—P—Cr alloy thin plate and a method for manufacturing the same. An embodiment of the present invention provides an Fe—P—Cr alloy thin plate including, in terms of wt %, P (6.0-13.0%), Cr (0.002-0.1%), and the balance of Fe and other inevitable impurities.

## Claims

### Claim at position 1

1-29. (canceled)

### Claim 30

An Fe—P—Cr alloy thin plate comprising, in terms of wt %, P (6.0-13.0%), Cr (0.002-0.1%), and the balance of Fe and other inevitable impurities.

### Claim 31 (depends on 30)

The Fe—P—Cr alloy thin plate of claim 30, wherein the Fe—P—Cr alloy thin plate further includes Ni (0.5-5.0%) in terms of wt %.

### Claim 32 (depends on 31)

The Fe—P—Cr alloy thin plate of claim 31, wherein the thin plate has Vickers hardness of less than or equal to 600 HV.

### Claim 33 (depends on 32)

The Fe—P—Cr alloy thin plate of claim 32, wherein the thin plate has a saturation magnetic flux density of greater than or equal to 1.5 T.

### Claim 34 (depends on 33)

The Fe—P—Cr alloy thin plate of claim 33, wherein the thin plate has a thickness of 1 μm to 100 μm.

### Claim 35 (depends on 34)

The Fe—P—Cr alloy thin plate of claim 34, wherein the Fe—P—Cr alloy thin plate has a mixed form of amorphous and crystal grains.

### Claim 36 (depends on 35)

The Fe—P—Cr alloy thin plate of claim 35, wherein the crystal grain has a particle diameter of greater than or equal to 0.1 nm and less than or equal to 100 nm.

### Claim 37 (depends on 36)

The Fe—P—Cr alloy thin plate of claim 36, wherein a volume fraction of the crystal grain based on an amorphous matrix is 1% to 10%.

### Claim 38

A method of manufacturing an Fe—P—Cr alloy thin plate, comprising:
forming a plating solution including an iron compound, a phosphorus compound, and a chromium compound;
applying a current to the formed plating solution;
electrodepositing an Fe—P—Cr alloy layer including, in terms of wt %, P (6.0-13.0%), Cr (0.002-0.1%), and the balance of Fe and other inevitable impurities on a cathode plate using the current; and
delaminating the Fe—P—Cr alloy layer from the cathode plate to obtain an Fe—P—Cr alloy thin plate.

### Claim 39 (depends on 38)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 38, wherein the Fe—P—Cr alloy thin plate has a thickness of 1 μm to 100 μm.

### Claim 40 (depends on 38)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 38, wherein the forming of the plating solution including the iron compound, the phosphorus compound, and the chromium compound includes
forming a plating solution including an iron compound, a phosphorus compound, a chromium compound, and a nickel compound.

### Claim 41 (depends on 40)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 40, wherein in the forming of the plating solution including the iron compound, the phosphorus compound, the chromium compound, and the nickel compound,
a concentration of the iron compound in the plating solution is 0.5 M to 4.0 M, and
the iron compound includes FeSO4, Fe(SO3NH2)2, FeCl2, or a combination thereof.

### Claim 42 (depends on 41)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 41, wherein in the forming of the plating solution including the iron compound, the phosphorus compound, the chromium compound, and the nickel compound,
a concentration of the phosphorus compound in the plating solution is 0.01 M to 3.0 M, and
the phosphorus compound includes NaH2PO2, H3PO2, H3PO3, or a combination thereof.

### Claim 43 (depends on 42)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 42, wherein in the forming of the plating solution including the iron compound, the phosphorus compound, the chromium compound, and the nickel compound,
a concentration of the chromium compound in the plating solution is 0.001 M to 2.0 M, and
the chromium compound includes CrCl3, Cr2(SO4)3, CrO3, or a combination thereof.

### Claim 44 (depends on 43)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 43, wherein in the forming of the plating solution including the iron compound, the phosphorus compound, the chromium compound, and the nickel compound,
a concentration of the nickel compound in the plating solution is 0.1 M to 3.0 M, and
the nickel compound includes NiSO4, NiCl2, or a combination thereof.

### Claim 45 (depends on 40)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 40, wherein the forming of the plating solution including the iron compound, the phosphorus compound, the chromium compound, and the nickel compound includes
forming a plating solution including the iron compound, the phosphorus compound, the chromium compound, the nickel compound, and an additive, wherein a concentration of the additive in the plating solution is 0.001 M to 0.1 M.

### Claim 46 (depends on 38)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 38, wherein in the forming of the plating solution including the iron compound, the phosphorus compound, and the chromium compound,
pH of the plating solution is 1 to 4.

### Claim 47 (depends on 38)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 38, wherein in the forming of the plating solution including the iron compound, the phosphorus compound, and the chromium compound,
a temperature of the plating solution is 30° C. to 100° C.

### Claim 48 (depends on 38)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 38, wherein in the applying of a current to the formed plating solution,
a current density is 1 A/dm2 to 100 A/dm2.

### Claim 49 (depends on 38)

The method of manufacturing an Fe—P—Cr alloy thin plate of claim 38, wherein the electrodepositing of the Fe—P—Cr alloy layer including, in terms of wt %, P (6.0-13.0%), Cr (0.002-0.1%), and the balance of Fe and other inevitable impurities on a cathode plate using the current includes
electrodepositing an Fe—P—Cr—Ni alloy layer including, in terms of wt %, P (6.0-13.0%), Cr (0.002-0.1%), Ni (0.5-5.0%), and the balance of Fe and other inevitable impurities on a cathode plate using the current.