# US 2017/0362678 A1 · High strength thick-walled electric-resistance-welded steel pipe for deep-well conductor casing, method for manufacturing the same, and high-strength thick-walled conductor casing for deep wells

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0362678 A1
- Document ID: US20170362678A1
- Status: Published application
- Kind: A1
- Application number: 15/539,510
- Filed: 2015-12-15
- Published: 2017-12-21
- Earliest claimed: 2014-12-25
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Sota GOTO; Takatoshi OKABE; Yukihiko OKAZAKI
- Web page: https://patentgrep.com/patent/US20170362678A1

## CPC

- C21D 9/50: for welded joints
- B21B 19/14: Rolling tubes by means of additional rollers arranged inside the tubes
- B21B 23/00: Tube-rolling not restricted to methods provided for in only one of groups B21B17/00, B21B19/00, B21B21/00, e.g. combined processes {planetary tube rolling, auxiliary arrangements, e.g. lubricating, special tube blanks, continuous casting combined with tube rolling}(B21B25/00 takes precedence)
- B21C 37/08: Making tubes with welded or soldered seams {(with helically arranged seams B21C37/122)}
- B23K 11/0873: {of the longitudinal seam of tubes}
- C21D 6/001: {containing Ni (C21D6/004 takes precedence)}
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0263: {following hot rolling}
- C21D 9/08: for tubular bodies or pipes
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- F16L 9/17: obtained by bending a sheet longitudinally and connecting the edges
- B23K 2101/06: Tubes
- B23K 2103/04: Steel {or steel} alloys
- C21D 2211/002: Bainite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- B21C: MANUFACTURE OF METAL SHEETS, WIRE, RODS, TUBES, PROFILES OR LIKE SEMI-MANUFACTURED PRODUCTS OTHERWISE THAN BY ROLLING; AUXILIARY OPERATIONS USED IN CONNECTION WITH METAL-WORKING WITHOUT ESSENTIALLY REMOVING MATERIAL
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F16L: PIPES; JOINTS OR FITTINGS FOR PIPES; SUPPORTS FOR PIPES, CABLES OR PROTECTIVE TUBING; MEANS FOR THERMAL INSULATION IN GENERAL

## Abstract

A high-strength high-toughness electric-resistance-welded steel pipe having high resistance to post-weld heat treatment is provided. The steel pipe having a composition including C: 0.01% to 0.12%, Si: 0.05% to 0.50%, Mn: 1.0% to 2.2%, P: 0.03% or less, S: 0.005% or less, Al: 0.001% to 0.10%, N: 0.006% or less, Nb: 0.010% to 0.100%, and Ti: 0.001% to 0.050%. The steel pipe having a structure composed of a 90% or more by volume of a bainitic ferrite phase as a main phase and 10% or less (including 0%) by volume of a second phase. The bainitic ferrite phase having an average grain size of 10 μm or less, and the structure containing fine Nb precipitates having a particle size of less than 20 nm dispersed in a base material portion. The steel pipe having high strength, toughness, and high resistance that is maintained through post-weld heat treatment.

## Claims

### Claim 1

A high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing,
the steel pipe having a composition comprising:
C: 0.01% to 0.12%, by mass %;
Si: 0.05% to 0.50%, by mass %;
Mn: 1.0% to 2.2%, by mass %;
P: 0.03% or less, by mass %;
S: 0.005% or less, by mass %;
Al: 0.001% to 0.10%, by mass %;
N: 0.006% or less, by mass %;
Nb: 0.010% to 0.100%, by mass %;
Ti: 0.001% to 0.050%, by mass %; and
Fe and incidental impurities,
wherein:
the steel pipe has a structure composed of 90% or more by volume of a bainitic ferrite phase as a main phase and 10% or less (including 0%) by volume of a second phase,
the bainitic ferrite phase having an average grain size of 10 μm or less, and
the structure containing fine Nb precipitates having a particle size of less than 20 nm dispersed in a base material portion, a ratio of fine Nb precipitates to a total amount of Nb being more than 75% on a Nb equivalent basis, and
a circularity of an end portion of the steel pipe defined by formula (1) being 0.6% or less,
circularity (%)={(maximum outer diameter mmφ of steel pipe)−(minimum outer diameter mmφ of steel pipe)}/(nominal outer diameter mmφ)×100 formula (1).

### Claim 2 (depends on 1)

The high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 1, wherein the composition comprises at least one of:
V: 0.1% or less, by mass %;
Mo: 0.5% or less, by mass %;
Cr: 0.5% or less, by mass %;
Cu: 0.5% or less, by mass %;
Ni: 1.0% or less, by mass % and
B: 0.0030% or less, by mass %.

### Claim 3 (depends on 1)

The high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 1, wherein the composition further comprises at least one of:
Ca: 0.0005% to 0.0050%, by mass %; and
REM: 0.0005% to 0.0050%, by mass %.

### Claim 4

A method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing, the method comprising:
continuously rolling a hot-rolled steel plate with a roll forming machine to form an open pipe having a generally circular cross section;
butting edges of the open pipe;
electric-resistance-welding a portion where the edges are being butted while pressing the butted edges to contact each other by squeeze rolls to form an electric-resistance-welded steel pipe;
subjecting the electric-resistance-welded portion of the electric-resistance-welded steel pipe to in-line heat treatment; and
reducing a diameter of the electric-resistance-welded steel pipe by rolling,
wherein:
the hot-rolled steel plate is manufactured by:
heating to soak a steel at a heating temperature in the range of 1150° C. to 1250° C. for 60 minutes or more,
hot-rolling the steel with a finishing delivery temperature of 750° C. or more,
after completion of the hot rolling, subjecting the hot-rolled steel plate to accerelated cooling such that an average cooling rate in a temperature range of 750° C. to 650° C. at the center of plate thickness ranges from 8° C./s to 70° C./s, and
coiling the hot-rolled steel plate at a coiling temperature of more than 580° C. and 700° C. or less,
the hot-rolled steel plate having a composition comprising:
C: 0.01% to 0.12%, by mass %,
Si: 0.05% to 0.50%, by mass %,
Mn: 1.0% to 2.2%, by mass %,
P: 0.03% or less, by mass %,
S: 0.005% or less, by mass %,
Al: 0.001% to 0.10%, by mass %,
N: 0.006% or less, by mass %,
Nb: 0.010% to 0.100%, by mass %,
Ti: 0.001% to 0.050%, by mass %, and
Fe and incidental impurities.

### Claim 5 (depends on 4)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 4, wherein the roll forming machine includes a cage roll group composed of a plurality of rolls and a fin pass forming roll group composed of a plurality of rolls.

### Claim 6 (depends on 5)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 5, wherein two or more portions of an inner wall of the hot-rolled steel plate are pressed with an inner roll disposed downstream of the cage roll group during a forming process.

### Claim 7 (depends on 4)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 4, wherein the in-line heat treatment of the electric-resistance-welded portion includes heating the electric-resistance-welded portion to a heating temperature in the range of 830° C. to 1150° C. and cooling the electric-resistance-welded portion to a cooling stop temperature of 550° C. or less at the center of the plate thickness such that an average cooling rate in a temperature range of 800° C. to 550° C. at the center of the plate thickness ranges from 10° C./s to 70° C./s.

### Claim 8 (depends on 4)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 4, wherein a reduction ratio in the reducing rolling is in the range of 0.2% to 3.3%.

### Claim 9 (depends on 4)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 4, wherein the composition further comprises at least one of:
V: 0.1% or less, by mass %,
Mo: 0.5% or less, by mass %,
Cr: 0.5% or less, by mass %,
Cu: 0.5% or less, by mass %,
Ni: 1.0% or less, by mass %, and
B: 0.0030% or less, by mass %.

### Claim 10 (depends on 4)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 4, wherein the composition further comprises at least one of:
Ca: 0.0005% to 0.0050%, by mass %, and
REM: 0.0005% to 0.0050%, by mass %.

### Claim 11 (depends on 1)

A high-strength thick-walled conductor casing for deep wells, the conductor casing comprising a screw member disposed on each end of the high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 1.

### Claim 12 (depends on 2)

The high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 2 wherein the composition further comprises at least one of:
Ca: 0.0005% to 0.0050%, by mass %; and
REM: 0.0005% to 0.0050%, by mass %.

### Claim 13 (depends on 7)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 7, wherein a reduction ratio in the reducing rolling is in the range of 0.2% to 3.3%.

### Claim 14 (depends on 7)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 7, wherein the composition further comprises at least one of:
V: 0.1% or less, by mass %,
Mo: 0.5% or less, by mass %,
Cr: 0.5% or less, by mass %,
Cu: 0.5% or less, by mass %,
Ni: 1.0% or less, by mass %, and
B: 0.0030% or less, by mass %.

### Claim 15 (depends on 8)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 8, wherein the composition further comprises at least one of:
V: 0.1% or less, by mass %,
Mo: 0.5% or less, by mass %,
Cr: 0.5% or less, by mass %,
Cu: 0.5% or less, by mass %,
Ni: 1.0% or less, by mass %, and
B: 0.0030% or less, by mass %.

### Claim 16 (depends on 7)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 7, wherein the composition further comprises at least one of:
Ca: 0.0005% to 0.0050%, by mass %; and
REM: 0.0005% to 0.0050%, by mass %.

### Claim 17 (depends on 8)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 8, wherein the composition further comprises at least one of:
Ca: 0.0005% to 0.0050%, by mass %; and
REM: 0.0005% to 0.0050%, by mass %.

### Claim 18 (depends on 9)

The method for manufacturing a high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 9, wherein the composition further comprises at least one of:
Ca: 0.0005% to 0.0050%, by mass %; and
REM: 0.0005% to 0.0050%, by mass %.

### Claim 19 (depends on 2)

A high-strength thick-walled conductor casing for deep wells, the conductor casing comprising a screw member disposed on each end of the high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 2.

### Claim 20 (depends on 3)

A high-strength thick-walled conductor casing for deep wells, the conductor casing comprising a screw member disposed on each end of the high-strength thick-walled electric-resistance-welded steel pipe for a deep-well conductor casing according to claim 3.