# US 2017/0292177 A1 · Thick-wall oil-well steel pipe and production method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0292177 A1
- Document ID: US20170292177A1
- Status: Published application
- Kind: A1
- Application number: 15/505,678
- Filed: 2015-08-31
- Published: 2017-10-12
- Earliest claimed: 2014-09-04
- Assignees: Nippon Steel & Sumitomo Metal Corporation
- Applicants: Nippon Steel & Sumitomo Metal Corporation
- Inventors: Yuji ARAI; Keiichi KONDO; Koji NAGAHASHI
- Web page: https://patentgrep.com/patent/US20170292177A1

## CPC

- C22C 38/44: with molybdenum or tungsten
- C21D 6/004: {containing Cr and Ni}
- C21D 9/08: for tubular bodies or pipes
- C21D 9/085: {Cooling or quenching}
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/54: with boron
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A thick-wall oil-well steel pipe has a wall thickness of 40 mm or more, excellent SSC resistance and high strength. The thick-wall oil-well steel pipe has a composition containing, in mass %, C: 0.40 to 0.65%, Si: 0.05 to 0.50%, Mn: 0.10 to 1.0%, P: 0.020% or less, S: 0.0020% or less, sol. Al: 0.005 to 0.10%, Cr more than 0.40 to 2.0%, Mo: more than 1.15 to 5.0%, Cu: 0.50% or less, Ni: 0.50% or less, N: 0.007% or less, and O: 0.005% or less. The number of carbide which has a circle equivalent diameter of 100 nm or more and contains 20 mass % or more of Mo is 2 or less per 100 mm2. The thick-wall oil-well steel pipe has yield strength of 827 MPa or more. A difference between a maximum value and a minimum value of the yield strength in the wall-thickness direction is 45 MPa or less.

## Claims

### Claim 1

A thick-wall oil-well steel pipe characterized by having a wall thickness of 40 mm or more, and having a chemical composition consisting of, in mass %,
C: 0.40 to 0.65%,
Si: 0.05 to 0.50%,
Mn: 0.10 to 1.0%,
P: 0.020% or less,
S: 0.0020% or less,
sol. Al: 0.005 to 0.10%,
Cr: more than 0.40 to 2.0%,
Mo: more than 1.15 to 5.0%,
Cu: 0.50% or less,
Ni: 0.50% or less,
N: 0.007% or less,
O: 0.005% or less,
V: 0 to 0.25%,
Nb: 0 to 0.10%,
Ti: 0 to 0.05%,
Zr: 0 to 0.10%,
W: 0 to 1.5%,
B: 0 to 0.005%,
Ca: 0 to 0.003%,
Mg: 0 to 0.003%, and
rare earth metal: 0 to 0.003%, with the balance being Fe and impurities, wherein
the number of carbide which has a circle equivalent diameter of 100 nm or more and contains 20 mass % or more of Mo is 2 or less per 100 μm2, and wherein
the thick-wall oil-well steel pipe has yield strength of 827 MPa or more, and a difference between a maximum value and a minimum value of the yield strength in a wall-thickness direction is 45 MPa or less.

### Claim 2 (depends on 1)

A method for producing a thick-wall oil-well steel pipe, characterized by comprising the steps of:
producing a steel pipe having the chemical composition according to claim 1,
subjecting the steel pipe to quenching once or multiple times, wherein a quenching temperature in the quenching of at least once is 925 to 1100° C., and
subjecting the steel pipe to tempering after the quenching.