# US 2017/0292176 A1 · Steel sheet for crown cap and method for producing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0292176 A1
- Document ID: US20170292176A1
- Status: Published application
- Kind: A1
- Application number: 15/518,190
- Filed: 2015-10-08
- Published: 2017-10-12
- Earliest claimed: 2014-10-10
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Masami TSUJIMOTO; Takumi TANAKA; Tomonari HIRAGUCHI; Katsumi KOJIMA; Makoto ARATANI; Reiko SUGIHARA; Fumio AOKI; Toshihiro KIKUCHI; Hiroki NAKAMARU
- Web page: https://patentgrep.com/patent/US20170292176A1

## CPC

- C22C 38/06: containing aluminium
- C21D 6/005: {containing Mn}
- C21D 8/0436: {Cold rolling}
- C21D 8/0468: {between cold rolling steps}
- C21D 9/46: for sheet metals
- C21D 9/48: deep-drawing sheets
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C21D 8/0426: {Hot rolling}
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A steel sheet for a crown cap having sufficient strength and formability suitable for forming crown caps even when reduced in gauge, and a method for producing the steel sheet for a crown cap. The steel sheet for a crown cap having a composition that includes, in terms of % by mass: C: 0.002% or more and 0.010% or less, Si: 0.05% or less, Mn: 0.05% or more and 0.30% or less, P: 0.030% or less, S: 0.020% or less, Al: less than 0.0100%, N: 0.0050% or less, and the balance being Fe and unavoidable impurities. The C content is more than 0.003% when the Al content is 0.005% or more. The yield strength in the rolling direction is 500 MPa or more. The average Lankford value is 1.3 or more.

## Claims

### Claim 1

A steel sheet for crown cap having a composition comprising, in terms of % by mass: C: 0.002% or more and 0.010% or less, Si: 0.05% or less, Mn: 0.05% or more and 0.30% or less, P: 0.030% or less, S: 0.020% or less, Al: less than 0.0100%, N: 0.0050% or less, and the balance being Fe and unavoidable impurities,
wherein the C content is more than 0.003% when the Al content is 0.005% or more,
a yield strength in a rolling direction is 500 MPa or more, and
an average Lankford value is 1.3 or more, in which
Average Lankford value=(rL+2×rD+rC)/4,
where rL represents a Lankford value in a direction parallel to the rolling direction, rD represents a Lankford value in a direction at 45° with respect to the rolling direction, and rC represents a Lankford value in a direction at 90° with respect to the rolling direction.

### Claim 2 (depends on 1)

The steel sheet for crown cap according to claim 1, wherein an absolute value of Δr is 0.40 or less, in which
Δr=(rL−2×rD+rC)/2,
where rL represents a Lankford value in a direction parallel to the rolling direction, rD represents a Lankford value in a direction at 45° with respect to the rolling direction, and rC represents a Lankford value in a direction at 90° with respect to the rolling direction.

### Claim 3 (depends on 1)

A method for producing a steel sheet for crown cap, the method comprising:
rough-rolling a slab having the composition according to claim 1 and finish-rolling the rough-rolled slab at a finish-rolling temperature of 850° C. or higher to obtain a hot-rolled sheet;
coiling the hot-rolled sheet at 450° C. or higher and 750° C. or lower to obtain a coiled sheet;
pickling the coiled sheet to obtain a pickled sheet;
cold-rolling the pickled sheet to obtain a cold-rolled sheet;
annealing the cold-rolled sheet at 650° C. or higher and 790° C. or lower to obtain an annealed sheet; and
cold-rolling the annealed sheet at a rolling reduction of 10% or more and 50% or less when the Al content is 0.003% or less or at a rolling reduction of 20% or more and 50% or less when the Al content is more than 0.003%.