# US 2017/0283901 A1 · Grade 550mpa high-temperature resistant pipeline steel and method of manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0283901 A1
- Document ID: US20170283901A1
- Status: Published application
- Kind: A1
- Application number: 15/512,209
- Filed: 2015-09-16
- Published: 2017-10-05
- Earliest claimed: 2014-09-19
- Assignees: Baoshan Iron & Steel Co., Ltd.
- Applicants: Baoshan Iron & Steel Co., Ltd.
- Inventors: Ping HU; Lei ZHENG; Chuanguo ZHANG
- Web page: https://patentgrep.com/patent/US20170283901A1

## CPC

- C21D 9/46: for sheet metals
- B21B 1/22: for rolling {plates, strips,} bands or sheets of indefinite length (B21B1/42 takes precedence)
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/58: with more than 1.5% by weight of manganese
- B21B 2001/225: {by hot-rolling}
- C21D 2211/004: Dispersions; Precipitations
- C21D 2211/005: Ferrite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

Disclosed is a Grade 550 MPa high temperature-resistant pipeline steel, the chemical elements, in mass percentage, being: 0.061%≦C≦0.120%, 1.70%≦Mn≦2.20%, 0.15%≦Mo≦0.39%, 0.15%≦Cu≦0.30%, 0.15%≦Ni≦0.50%, 0.035%≦Nb≦0.080%, 0.005%≦V≦0.054%, 0.005%≦Ti≦0.030%, 0.015%≦Al≦0.040%, 0.005%≦Ca≦0.035%, and the balance being Fe and unavoidable impurities. Also disclosed is a manufacturing method of the Grade 550 MPa high temperature-resistant pipeline steel, comprising the steps of: smelting, casting, slab heating, rough rolling, finish rolling, controlled cooling, and air cooling to room temperature. The pipeline steel has an excellent mechanical property under a high temperature.

## Claims

### Claim 1

A Grade 550 MPa high-temperature resistant pipeline steel, the chemical elements thereof, in mass percentages, being: 0.061%≦C≦0.120%; 1.70%≦Mn≦2.20%; 0.15%≦Mo≦0.39%; 0.15%≦Cu≦0.30%; 0.15%≦Ni≦0.50%; 0.035%≦Nb≦0.080%; 0.005%≦V≦0.054%; 0.005%≦Ti≦0.030%; 0.015%≦Al≦0.040%; 0.005%≦Ca≦0.035%, and the balance being Fe and unavoidable impurities.

### Claim 2 (depends on 1)

The Grade 550 MPa high-temperature resistant pipeline steel according to claim 1, further comprising at least one of O<Si≦0.40%, O<Cr≦0.40% and 021 N≦0.005%.

### Claim 3 (depends on 1)

The Grade 550 MPa high-temperature resistant pipeline steel according to claim 1, wherein the Grade 550 MPa high-temperature resistant pipeline steel has a microstructure comprising homogeneous needle-shaped ferrite structure+a matrix formed from a small amount of M-A component.

### Claim 4

The Grade 550 MPa high-temperature resistant pipeline steel of according to 3, wherein the M-A component has a volumetric percentage ≦10%.

### Claim 5 (depends on 3)

The Grade 550 MPa high-temperature resistant pipeline steel according to claim 3, wherein the matrix has an average effective grain size ≦8 μm.

### Claim 6 (depends on 5)

The Grade 550 MPa high-temperature resistant pipeline steel according to claim 5, wherein the matrix has a volumetric percentage of a small angle grain boundary of 20-60%.

### Claim 7 (depends on 3)

The Grade 550 MPa high-temperature resistant pipeline steel according to claim 3, wherein precipitated carbides NbC, VC and carbonitrides (Nb, V) (C, N) formed from Nb and V are dispersively distributed on the matrix.

### Claim 8 (depends on 7)

The Grade 550 MPa high-temperature resistant pipeline steel according to claim 7, wherein the carbides and carbonitrides have an average size of 5-50 nm.

### Claim 9 (depends on 1)

A method of manufacturing the Grade 550 MPa high-temperature resistant pipeline steel of any one of claim 1, comprising the following steps: smelting; casting; slab heating; rough rolling; finish rolling; controlled cooling; and air cooling to room temperature.

### Claim 10 (depends on 9)

The method of manufacturing the Grade 550 MPa high-temperature resistant pipeline steel according to claim 9, wherein in the rough rolling step, an initial rolling temperature of the rough rolling is 1100-1180° C., and an end rolling temperature of the rough rolling is 950-980° C.

### Claim 11 (depends on 9)

The method of manufacturing the Grade 550 MPa high-temperature resistant pipeline steel according to claim 9, wherein in the finish rolling step, an initial rolling temperature of the finish rolling is 850-900° C.; an end rolling temperature of the finish rolling is 800-820° C.; and a finish rolling compression ratio is 4T-8T, wherein T is a thickness of a final steel plate.

### Claim 12 (depends on 9)

The method of manufacturing the Grade 550 MPa high-temperature resistant pipeline steel according to claim 9, wherein in the controlled cooling step, an initial cooling temperature is 750-780° C.; a cooling rate is 15-30° C/s; and an end cooling temperature is 380-580° C.

### Claim 13 (depends on 9)

The method of manufacturing the Grade 550 MPa high-temperature resistant pipeline steel according to claim 9, wherein in the slab heating step, a heating temperature is 1110-1250° C.