# US 2017/0253957 A1 · Method of producing a nitrided packaging steel

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0253957 A1
- Document ID: US20170253957A1
- Status: Published application
- Kind: A1
- Application number: 15/506,911
- Filed: 2015-07-02
- Published: 2017-09-07
- Earliest claimed: 2014-08-27
- Assignees: thyssenkrupp Rasselstein GmbH; thyssenkrupp AG
- Applicants: ThyssenKrupp Rasselstein GmbH; ThyssenKrupp AG
- Inventors: Burkhard KAUP; Blaise MASSICOT; Dirk MATUSCH
- Web page: https://patentgrep.com/patent/US20170253957A1

## CPC

- C23C 8/26: of ferrous surfaces
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0236: {Cold rolling}
- C21D 8/0257: {with diffusion of elements, e.g. decarburising, nitriding}
- C21D 8/04: to produce plates or strips for drawing, e.g. for deep-drawing
- C21D 8/0436: {Cold rolling}
- C21D 8/0457: {with diffusion of elements, e.g. decarburising, nitriding}
- C21D 8/0473: {Final recrystallisation annealing}
- C21D 9/48: deep-drawing sheets
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C23C 8/80: After-treatment
- C23F 17/00: Multi-step processes for surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by subclass C21D or C22F or class C25 (coating for obtaining at least two superposed coatings either by methods not provided for in a single one of main groups C23C2/00 - C23C26/00, or by combinations of methods providedfor in subclasses C23C and C25D, C23C28/00)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23F: NON-MECHANICAL REMOVAL OF METALLIC MATERIAL FROM SURFACE (working metal by laser beams B23K26/00; desurfacing by applying flames B23K7/00; working of metal by electro-erosion B23H; producing decorative effects by removing surface material, e.g. by engraving, by etching, B44C1/22; electrolytic etching or polishing C25F); INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL; MULTI-STEP PROCESSES FOR SURFACE TREATMENT OF METALLIC MATERIAL INVOLVING AT LEAST ONE PROCESS PROVIDED FOR IN CLASS C23 AND AT LEAST ONE PROCESS COVERED BY SUBCLASS C21D OR C22F OR CLASS C25

## Abstract

A nitrided packaging steel in the form of a flat steel product and method for producing a nitrided packaging steel with a carbon content of 10-1000 ppm and uncombined nitrogen, dissolved in the steel, of more than 100 ppm. The nitriding is performed in two stages: a first stage, in which a molten steel is nitrided to a nitrogen content of at most 160 ppm by introducing a nitrogen-containing gas and/or a nitrogen-containing solid into the molten steel, and a second stage, in which a flat steel product produced from the nitrided molten steel by cold rolling is treated with a nitrogen-containing gas in order to increase further the amount of uncombined nitrogen in the flat steel product. The second stage is performed in an annealing furnace, in which the flat steel product is at the same time annealed in a recrystallizing manner. The packaging steels produced are distinguished by great strength, in excess of 600 MPa, and good elongation to fracture, regularly in excess of 5%, as well as by good forming properties.

## Claims

### Claim 1

A method of producing a nitrided packaging steel with a carbon content of 10 to 1000 ppm and a quantity of uncombined nitrogen dissolved in the steel of more than 100 ppm, the method comprising:
a) nitriding a molten steel to a nitrogen content of a maximum of 160 ppm by feeding a nitrogen-containing gas and/or a nitrogen-containing solid into the molten steel;
b) casting a slab from the molten steel and hot rolling the slab to form a hot strip;
c) cold rolling the hot strip to form a flat steel product;
d) recrystallization annealing the cold-rolled flat steel product in an annealing furnace, in particular a continuous annealing furnace, wherein a nitrogen-containing gas is introduced into the annealing furnace and directed onto the flat steel product so as to further increase the quantity of uncombined nitrogen in the flat steel product.

### Claim 2 (depends on 1)

The method as in claim 1, wherein in Step a), nitriding of the molten steel takes place by feeding nitrogen gas (N2) and/or calcium cyanamide (CaCN2) and/or manganese nitride (MnN) into the molten steel.

### Claim 3 (depends on 1)

The method as in claim 1 wherein in Step d), ammonia gas (NH3) is fed into the annealing furnace.

### Claim 4 (depends on 3)

The method as in claim 3, wherein the ammonia gas (NH3) in the annealing furnace is directed onto the flat steel product by means of one or a plurality of spray nozzles.

### Claim 5 (depends on 3)

The method as in claim 3, wherein as a result of feeding in the ammonia gas (NH3), an ammonia equilibrium with a concentration in the range of 0.05 to 1.5% is established in the annealing furnace.

### Claim 6 (depends on 3)

The method as in claim 3, wherein the ammonia equilibrium concentration resulting in the annealing furnace as a result of feeding in ammonia gas (NH3) is measured by means of an ammonia sensor.

### Claim 7 (depends on 6)

The method as in claim 6, wherein the value of the ammonia equilibrium concentration measured is used to control the quantity of ammonia gas fed per unit of time into the annealing furnace.

### Claim 8 (depends on 3)

The method as in claim 3, wherein in addition to ammonia gas (NH3), an inert gas, in particular nitrogen gas (N2) and/or hydrogen gas (H2), preferably a mixture of 95 wt % of nitrogen gas (N2) and 5 wt % of hydrogen gas (H2), is also fed into the annealing furnace.

### Claim 9 (depends on 1)

The method as in claim 1, wherein after nitriding the cold-rolled flat steel product in the annealing furnace, the quantity of uncombined nitrogen is in a range of 100 to 500 ppm, preferably more than 150 ppm, and most preferably in a range of 200 to 350 ppm.

### Claim 10 (depends on 1)

The method as in claim 1, wherein the recrystallization annealing of the cold-rolled flat steel product in Step d) is accomplished by passing the flat steel product through continuous annealing furnace in which the flat steel product is heated to temperatures of more than 600° C. and preferably to a temperature in a range of 620° C. to 660° C.

### Claim 11 (depends on 1)

The method as in claim 1, wherein the carbon content of the steel is in a range of 100 to 1000 ppm and preferably in a range of 500 to 900 ppm.

### Claim 12 (depends on 1)

A nitrided packaging steel in the form of a flat steel product having a thickness of less than 0.5 mm and preferably of less than 0.4 mm, especially produced by the method as in claim 1, with the packaging steel having a carbon content in a range of 10 to 1000 ppm and an average quantity of uncombined nitrogen dissolved in the steel of more than 100 ppm, wherein the concentration distribution of the uncombined nitrogen varies from the mean quantity of nitrogen by less than ±10 ppm throughout the thickness of the flat steel product.

### Claim 13 (depends on 12)

The nitrided packaging steel as in claim 12, wherein the concentration distribution of the uncombined nitrogen varies from the mean quantity of nitrogen by less than ±5 ppm throughout the thickness of flat steel products.

### Claim 14 (depends on 12)

The nitrided packaging steel as in claim 12, wherein the ultimate tensile strength of the packaging steel is greater than 600 MPa.

### Claim 15 (depends on 12)

The nitrided packaging steel as in claim 12, wherein the mean quantity of uncombined nitrogen is greater than 150 ppm and preferably in a range of 200 and 350 ppm.