# US 2017/0253954 A1 · Aluminum alloy wire rod, aluminum alloy stranded wire, covered wire, wire harness, and method of manufacturing aluminum alloy wire rod

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0253954 A1
- Document ID: US20170253954A1
- Status: Published application
- Kind: A1
- Application number: 15/599,658
- Filed: 2017-05-19
- Published: 2017-09-07
- Earliest claimed: 2014-12-05
- Assignees: Furukawa Electric Co., Ltd.; Furukawa Automotive Systems Inc.
- Applicants: Furukawa Electric Co., Ltd.; Furukawa Automotive Systems Inc.
- Inventors: Sho YOSHIDA; Shigeki SEKIYA; Kengo MITOSE
- Web page: https://patentgrep.com/patent/US20170253954A1

## CPC

- C22F 1/04: of aluminium or alloys based thereon
- C22C 21/02: with silicon as the next major constituent
- C22C 21/08: with silicon
- C22F 1/00: Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working (apparatus for mechanical working of metal B21, B23, B24)
- C22F 1/043: of alloys with silicon as the next major constituent
- H01B 1/023: {Alloys based on aluminium}
- H01B 5/02: Single bars, rods, wires, or strips
- H01B 5/08: Several wires or the like stranded in the form of a rope
- H01B 7/0045: {Cable-harnesses}
- H01B 7/02: Disposition of insulation
- H01B 13/0016: {for heat treatment}
- H01B 13/0036: {Details}
- H01R 11/11: End pieces or tapping pieces for wires, supported by the wire and for facilitating electrical connection to some other wire, terminal or conductive member (H01R11/01 takes precedence)
- B21C 1/003: {Drawing materials of special alloys so far as the composition of the alloy requires or permits special drawing methods or sequences}
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01B: CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES (selection for magnetic properties H01F1/00; waveguides H01P {; printed circuits H05K})
- H01R: ELECTRICALLY-CONDUCTIVE CONNECTIONS; STRUCTURAL ASSOCIATIONS OF A PLURALITY OF MUTUALLY-INSULATED ELECTRICAL CONNECTING ELEMENTS; COUPLING DEVICES; CURRENT COLLECTORS
- B21C: MANUFACTURE OF METAL SHEETS, WIRE, RODS, TUBES, PROFILES OR LIKE SEMI-MANUFACTURED PRODUCTS OTHERWISE THAN BY ROLLING; AUXILIARY OPERATIONS USED IN CONNECTION WITH METAL-WORKING WITHOUT ESSENTIALLY REMOVING MATERIAL

## Abstract

An aluminum alloy wire rod includes Mg: 0.1-1.0 mass %, Si: 0.1-1.2 mass %, Fe: 0.10-1.40 mass %, Ti: 0-0.100 mass %, B: 0-0.030 mass %, Cu: 0-1.00 mass %, Ag: 0-0.50 mass %, Au: 0-0.50 mass %, Mn: 0-1.00 mass %, Cr: 0-1.00 mass %, Zr: 0-0.50 mass %, Hf: 0-0.50 mass %, V: 0-0.50 mass %, Sc: 0-0.50 mass %, Co: 0-0.50 mass %, Ni: 0-0.50 mass %, and the balance: Al and inevitable impurities. In a cross section parallel to a wire rod lengthwise direction and including a center line of the wire rod, no void having an area greater than 20 μm2 is present, or even in a case where at least one void having an area greater than 20 μm2 is present, a presence ratio of the at least one void per 1000 μm2 is on average in a range of less than or equal to one void/1000 μm2.

## Claims

### Claim 1

An aluminum alloy wire rod comprising Mg: 0.1 mass % to 1.0 mass %, Si: 0.1 mass % to 1.2 mass %, Fe: 0.10 mass % to 1.40 mass %, Ti: 0 mass % to 0.100 mass %, B: 0 mass % to 0.030 mass %, Cu: 0 mass % to 1.00 mass %, Ag: 0 mass % to 0.50 mass %, Au: 0 mass % to 0.50 mass %, Mn: 0 mass % to 1.00 mass %, Cr: 0 mass % to 1.00 mass %, Zr: 0 mass % to 0.50 mass %, Hf: 0 mass % to 0.50 mass %, V: 0 mass % to 0.50 mass %, Sc: 0 mass % to 0.50 mass %, Co: 0 mass % to 0.50 mass %, Ni: 0 mass % to 0.50 mass %, and the balance: Al and inevitable impurities,
wherein in a cross section parallel to a wire rod lengthwise direction and including a center line of the wire rod, no void having an area greater than 20 μm2 is present, or even in a case where at least one void having an area greater than 20 μm2 is present, a presence ratio of the at least one void per 1000 μm2 is on average in a range of less than or equal to one void/1000 μm2.

### Claim 2 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein in the cross section, no void having an area greater than 1 μm2 is present, or even in a case where at least one void having an area greater than 1 μm2 is present, a presence ratio of the at least one void per 1000 μm2 is on average in a range of less than or equal to one void/1000 μm2.

### Claim 3 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein in the cross section, no Fe-based compound particle having an area of greater than 4 μm2 is present, or even in a case where at least one Fe-based compound particle having an area of greater than 4 μm2 is present, a presence ratio of the at least one Fe-based compound particles per 1000 μm2 is on average in a range of less than or equal to one particle/1000 μm2.

### Claim 4 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein in the cross section, a presence ratio of at least one Fe-based compound particle having an area of 0.002 to 1 μm2 is on average in a range of greater than or equal to one particle/1000 μm2.

### Claim 5 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein in a case where at least 1000 crystal grains are observed in a metal structure, an average presence probability of at least one crystal grain having a maximum dimension in the diameter direction of the wire rod that is greater than or equal to half of the diameter of the wire rod is less than 0.10%.

### Claim 6 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein number of cycles of vibration to fracture is greater than or equal to 2,000,000 cycles, number cycles of bending to fracture is greater than or equal to 200,000 cycles and conductivity is greater than or equal to 40% IACS.

### Claim 7 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein the aluminum alloy wire rod comprises both of or any one of Ti: 0.001 mass % to 0.100 mass % and B: 0.001 mass % to 0.030 mass %.

### Claim 8 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein the aluminum alloy wire rod comprises at least one of Cu: 0.01 mass % to 1.00 mass %, Ag: 0.01 mass % to 0.50 mass %, Au: 0.01 mass % to 0.50 mass %, Mn: 0.01 mass % to 1.00 mass %, Cr: 0.01 mass % to 1.00 mass %, Zr: 0.01 mass % to 0.50 mass %, Hf: 0.01 mass % to 0.50 mass %, V: 0.01 mass % to 0.50 mass %, Sc: 0.01 mass % to 0.50 mass %, Co: 0.01 mass % to 0.50 mass % and Ni: 0.01 mass % to 0.50 mass %.

### Claim 9 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein the aluminum alloy wire rod comprises Ni: 0.01 mass % to 0.50 mass %.

### Claim 10 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein a sum of contents of Fe, Ti, B, Cu, Ag, Au, Mn, Cr, Zr, Hf, V, Sc, Co and Ni is 0.10 mass % to 2.00 mass %.

### Claim 11 (depends on 1)

The aluminum alloy wire rod according to claim 1, wherein the aluminum alloy wire rod is an aluminum alloy wire having a strand diameter of 0.1 mm to 0.5 mm.

### Claim 12 (depends on 11)

An aluminum alloy stranded wire obtained by stranding a plurality of the aluminum alloy wires as claimed in claim 11.

### Claim 13 (depends on 11)

A covered wire comprising a covering layer at an outer periphery of one of the aluminum alloy wire as claimed in claim 11.

### Claim 14

A wire harness comprising:
a covered wire including a covering layer at an outer periphery of one of an aluminum alloy wire rod and an aluminum alloy stranded wire; and
a terminal fitted at an end portion of the covered wire, the covering layer being removed from the end portion,
wherein the aluminum alloy wire rod comprises Mg: 0.1 mass % to 1.0 mass %, Si: 0.1 mass % to 1.2 mass %, Fe: 0.10 mass % to 1.40 mass %, Ti: 0 mass % to 0.100 mass %, B: 0 mass % to 0.030 mass %, Cu: 0 mass % to 1.00 mass %, Ag: 0 mass % to 0.50 mass %, Au: 0 mass % to 0.50 mass %, Mn: 0 mass % to 1.00 mass %, Cr: 0 mass % to 1.00 mass %, Zr: 0 mass % to 0.50 mass %, Hf: 0 mass % to 0.50 mass %, V: 0 mass % to 0.50 mass %, Sc: 0 mass % to 0.50 mass %, Co: 0 mass % to 0.50 mass %, Ni: 0 mass % to 0.50 mass %, and the balance: Al and inevitable impurities,
wherein in a cross section parallel to a wire rod lengthwise direction and including a center line of the wire rod, no void having an area greater than 20 μm2 is present, or even in a case where at least one void having an area greater than 20 μm2 is present, a presence ratio of the at least one void per 1000 μm2 is on average in a range of less than or equal to one void/1000 μm2.

### Claim 15

A method of manufacturing an aluminum alloy wire rod comprising:
forming a drawing stock through hot working subsequent to melting and casting an aluminum alloy material having a composition comprising Mg: 0.1 mass % to 1.0 mass %, Si: 0.1 mass % to 1.2 mass %, Fe: 0.10 mass % to 1.40 mass %, Ti: 0 mass % to 0.100 mass %, B: 0 mass % to 0.030 mass %, Cu: 0 mass % to 1.00 mass %, Ag: 0 mass % to 0.50 mass %, Au: 0 mass % to 0.50 mass %, Mn: 0 mass % to 1.00 mass %, Cr: 0 mass % to 1.00 mass %, Zr: 0 mass % to 0.50 mass %, Hf: 0 mass % to 0.50 mass %, V: 0 mass % to 0.50 mass %, Sc: 0 mass % to 0.50 mass %, Co: 0 mass % to 0.50 mass %, Ni: 0 mass % to 0.50 mass %, and the balance: Al and inevitable impurities; and
subsequently, performing steps including at least a wire drawing step, a solution heat treatment and an aging heat treatment,
wherein in the wire drawing step, wire drawing is performed with a maximum line tension of 50 N or less until a wire size of the wire rod reaches a final wire size from a wire size of twice the final wire size to the final wire size;
the solution heat treatment includes heating at a predetermined temperature in a range of 450° C. to 580° C., retaining at the predetermined temperature for a predetermined time, and thereafter cooling at an average cooling rate of greater than or equal to 10° C./s to at least a temperature of 150° C.; and
the aging heat treatment includes heating at a predetermined temperature of 20° C. to 250° C.

### Claim 16 (depends on 15)

The method of manufacturing an aluminum alloy wire rod according to claim 15, wherein an average cooling rate from the molten metal temperature to 400° C. in the casting is 20° C./sec to 50° C./sec; a re-heat treatment is performed after the casting and before the wire drawing process; and the re-heat treatment includes a heating at a predetermined temperature of higher than or equal to 400° C., and a retaining at the predetermined temperature for a period of time of less than or equal to 30 minutes.

### Claim 17 (depends on 12)

A covered wire comprising a covering layer at an outer periphery of the aluminum alloy stranded wire as claimed in claim 12.