# US 2017/0253943 A1 · Method and facility for producing high-strength galavanized steel sheets

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2017/0253943 A1
- Document ID: US20170253943A1
- Status: Published application
- Kind: A1
- Application number: 15/509,353
- Filed: 2015-08-20
- Published: 2017-09-07
- Earliest claimed: 2014-09-08
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Yoichi MAKIMIZU; Yoshitsugu SUZUKI; Hideyuki TAKAHASHI; Gentaro TAKEDA; Koichiro FUJITA
- Web page: https://patentgrep.com/patent/US20170253943A1

## CPC

- C21D 9/46: for sheet metals
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/18: containing chromium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- C23C 2/0038: {characterised by the pre-treatment chambers located immediately upstream of the bath or occurring locally before the dipping process}
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0222: {in a reactive atmosphere, e.g. oxidising or reducing atmosphere (C23C2/024 takes precedence)}
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/40: Plates; Strips
- C23F 17/00: Multi-step processes for surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by subclass C21D or C22F or class C25 (coating for obtaining at least two superposed coatings either by methods not provided for in a single one of main groups C23C2/00 - C23C26/00, or by combinations of methods providedfor in subclasses C23C and C25D, C23C28/00)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C23F: NON-MECHANICAL REMOVAL OF METALLIC MATERIAL FROM SURFACE (working metal by laser beams B23K26/00; desurfacing by applying flames B23K7/00; working of metal by electro-erosion B23H; producing decorative effects by removing surface material, e.g. by engraving, by etching, B44C1/22; electrolytic etching or polishing C25F); INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL; MULTI-STEP PROCESSES FOR SURFACE TREATMENT OF METALLIC MATERIAL INVOLVING AT LEAST ONE PROCESS PROVIDED FOR IN CLASS C23 AND AT LEAST ONE PROCESS COVERED BY SUBCLASS C21D OR C22F OR CLASS C25

## Abstract

A method for producing high-strength galvanized steel sheets having excellent coating adhesion, workability and appearance. The method comprises hot rolling a slab comprising, by mass %, C: 0.05 to 0.30%, Si: 0.1 to 2.0% and Mn: 1.0 to 4.0%, then coiling the steel sheet into a coil at a specific temperature TC, and pickling the steel sheet, cold rolling the hot-rolled steel sheet resulting from the hot rolling, annealing the cold-rolled steel sheet resulting from the cold rolling under specific conditions, and galvanizing the annealed sheet resulting from the annealing in a galvanizing bath containing 0.12 to 0.22 mass % Al.

## Claims

### Claim 1

A method for producing high-strength galvanized steel sheets, the method comprising:
hot rolling a slab comprising, by mass %, C: 0.05 to 0.30%, Si: 0.1 to 2.0% and Mn: 1.0 to 4.0%, into a steel sheet, then coiling the steel sheet into a coil at a temperature TC satisfying the relationship (1), and pickling the steel sheet;
cold rolling the hot-rolled steel sheet resulting from the hot rolling;
annealing the cold-rolled steel sheet resulting from the cold rolling, the annealing including (zone-A heating), (zone-B heating), and (zone-C heating); and
galvanizing the annealed sheet resulting from the annealing in a galvanizing bath comprising 0.12 to 0.22 mass % Al, wherein:
(zone-A heating): the cold-rolled steel sheet is heated in a DFF heating furnace at an air ratio α and an average heating rate at 200° C. and above is in a range of 10 to 50° C./sec to a target heating temperature T1 (° C.) satisfying the relationship (2),
(zone-B heating): the cold-rolled steel sheet resulting from the zone-A heating is heated in a DFF heating furnace at an air ratio ≦0.9 and an average heating rate at above T1 is in a range of 5 to 30° C./sec to a target heating temperature T2 (° C.) satisfying the relationship (3), and
(zone-C heating): the cold-rolled steel sheet resulting from the zone-B heating is heated in an atmosphere containing H2 and H2O, the balance being N2 and inevitable impurities, at a log(PH2O/PH2) in a range of not less than −3.4 and not more than −1.1 and an average heating rate at above T2 is in a range of 0.1 to 10° C./sec to a prescribed target heating temperature T3 (° C.) in a range of 700 to 900° C., and is held at T3 for 10 to 500 seconds,
TC≦−60([Si]+[Mn])+775 (1)
T1≧28.2[Si]+7.95[Mn]−86.2α+666 (2)
T2≧T1+30 (3)
wherein [Si] and [Mn] are the contents of mass % Si and Mn present in the slab, a is not more than 1.5, and log(PH2O/PH2) is log(H2O partial pressure (PH2O)/H2 partial pressure (PH2)).

### Claim 2 (depends on 1)

The method for producing high-strength galvanized steel sheets according to claim 1, wherein in the hot-rolled steel sheet obtained in the hot rolling, the total amount of internal Si oxide and internal Mn oxide found in a subsurface region of the steel sheet at a depth of not more than 10 μm from the steel sheet surface is not more than 0.10 g/m2 per side as expressed in terms of an amount of oxygen in a portion at a central position of the coil of the hot-rolled steel sheet in the longitudinal direction and in the width direction.

### Claim 3 (depends on 1)

The method for producing high-strength galvanized steel sheets according to claim 1, wherein a burner of the DFF heating furnace for the zone-A heating is a nozzle mix burner, and
a burner of the DFF heating furnace for the zone-B heating is a premix burner.

### Claim 4 (depends on 1)

The method for producing high-strength galvanized steel sheets according to claim 1, wherein log(PH2O/PH2) in the zone-C heating satisfies the relationship (4),
0.6[Si]−3.4≦log(PH2O/PH2)≦0.8[Si]−2.7 (4)
wherein [Si] is the mass % Si content in the steel.

### Claim 5 (depends on 1)

The method for producing high-strength galvanized steel sheets according to claim 1, comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 6 (depends on 1)

The method for producing high-strength galvanized steel sheets according to claim 1, further comprising cooling the steel sheet after the zone-C heating from 750° C. to a prescribed target cooling temperature T4 (° C.) in a range of 150 to 350° C. at an average cooling rate of not less than 10° C./sec, thereafter heating the steel sheet to a prescribed reheating temperature T5 (° C.) in a range of 350 to 600° C., and holding the steel sheet at the temperature T5 for 10 to 600 seconds.

### Claim 7

A continuous galvanizing production facility for manufacturing high-strength galvanized steel sheets, the facility comprising:
a DFF heating furnace having an upstream nozzle mix burner and a downstream premix burner; and
a radiant tube soaking furnace.

### Claim 8 (depends on 2)

The method for producing high-strength galvanized steel sheets according to claim 2, wherein a burner of the DFF heating furnace for the zone-A heating is a nozzle mix burner, and
a burner of the DFF heating furnace for the zone-B heating is a premix burner.

### Claim 9 (depends on 2)

The method for producing high-strength galvanized steel sheets having excellent appearance and coating adhesion according to claim 2, wherein log(PH2O/PH2) in the zone-C heating satisfies the relationship (4),
0.6[Si]−3.4≦log(PH2O/PH2)≦0.8[Si]−2.7 (4)
wherein [Si] is the mass % Si content in the steel.

### Claim 10 (depends on 3)

The method for producing high-strength galvanized steel sheets having excellent appearance and coating adhesion according to claim 3, wherein log(PH2O/PH2) in the zone-C heating satisfies the relationship (4),
0.6[Si]−3.4≦log(PH2O/PH2)≦0.8[Si]−2.7 (4)
wherein [Si] is the mass % Si content in the steel.

### Claim 11 (depends on 8)

The method for producing high-strength galvanized steel sheets having excellent appearance and coating adhesion according to claim 8, wherein log(PH2O/PH2) in the zone-C heating satisfies the relationship (4),
0.6[Si]−3.4≦log(PH2O/PH2)≦0.8[Si]−2.7 (4)
wherein [Si] is the mass % Si content in the steel.

### Claim 12 (depends on 2)

The method for producing high-strength galvanized steel sheets according to claim 2, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 13 (depends on 3)

The method for producing high-strength galvanized steel sheets according to claim 3, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 14 (depends on 4)

The method for producing high-strength galvanized steel sheets according to claim 4, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 15 (depends on 8)

The method for producing high-strength galvanized steel sheets according to claim 8, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 16 (depends on 9)

The method for producing high-strength galvanized steel sheets according to claim 9, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 17 (depends on 10)

The method for producing high-strength galvanized steel sheets according to claim 10, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 18 (depends on 11)

The method for producing high-strength galvanized steel sheets according to claim 11, further comprising alloying the steel sheet resulting from the galvanizing at an alloying temperature Ta satisfying the relationship (5) for 10 to 60 seconds,
−45 log(PH2O/PH2)+395≦Ta≦−30 log(PH2O/PH2)+490 (5)
wherein the galvanizing bath includes 0.12 to 0.17 mass % Al.

### Claim 19 (depends on 2)

The method for producing high-strength galvanized steel sheets according to claim 2, further comprising cooling the steel sheet after the zone-C heating from 750° C. to a prescribed target cooling temperature T4 (° C.) in a range of 150 to 350° C. at an average cooling rate of not less than 10° C./sec, thereafter heating the steel sheet to a prescribed reheating temperature T5 (° C.) in a range of 350 to 600° C., and holding the steel sheet at the temperature T5 for 10 to 600 seconds.

### Claim 20 (depends on 3)

The method for producing high-strength galvanized steel sheets according to claim 3, further comprising cooling the steel sheet after the zone-C heating from 750° C. to a prescribed target cooling temperature T4 (° C.) in a range of 150 to 350° C. at an average cooling rate of not less than 10° C./sec, thereafter heating the steel sheet to a prescribed reheating temperature T5 (° C.) in a range of 350 to 600° C., and holding the steel sheet at the temperature T5 for 10 to 600 seconds.