# US 2016/0355655 A1 · Bimodal Propylene Polymers and Sequential Polymerization

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0355655 A1
- Document ID: US20160355655A1
- Status: Published application
- Kind: A1
- Application number: 15/142,268
- Filed: 2016-04-29
- Published: 2016-12-08
- Earliest claimed: 2015-06-05
- Assignees: ExxonMobil Chemical Patents Inc.
- Applicants: ExxonMobil Chemical Patents Inc.
- Inventors: Luo Lubin; Matthew W. Holtcamp; Gregory S. Day
- Web page: https://patentgrep.com/patent/US20160355655A1

## CPC

- C08F 110/06: Propene
- C08F 4/02: Carriers therefor
- C08F 4/65912: {in combination with an organoaluminium compound}
- C08F 4/65916: {supported on a carrier, e.g. silica, MgCl2, polymer}
- C08F 10/06: Propene
- C08F 210/06: Propene
- C08L 23/12: Polypropene
- C08F 4/65927: {two cyclopentadienyl rings being mutually bridged}
- C08F 2410/06: Catalyst characterized by its size
- C08F 2420/09: Cyclic bridge, i.e. Cp or analog where the bridging unit linking the two Cps or analogs is part of a cyclic group
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)

## Abstract

This invention relates to high porosity (≧15%) and/or low pore diameter (PD<165 μm) propylene polymers and propylene polymerization processes using single site catalyst systems with supports having high surface area (SA≧400 m2/g), low pore volume (PV≦2 mL/g), a specific mean pore diameter range (PD=1-20 nm), and high average particle size (PS≧30 μm).

## Claims

### Claim 1

A process to polymerize propylene comprising:
(a) contacting propylene monomer under polymerization conditions with a catalyst system comprising a single site catalyst precursor compound, an activator, and a support comprising an average particle size of more than 30 μm, a surface area of 400 m2/g or more, a pore volume of from 0.5 to 2 mL/g, and a mean pore diameter of from 1 to 20 nm (10 to 200 Å);
(b) polymerizing the propylene in (a) for a time period, Al to form a first mode of propylene polymer comprising at least 50 mol % propylene;
(c) adding hydrogen or other chain transfer agent and optional comonomer to the polymerization after time period A1;
(d) then polymerizing the propylene in (a) in the presence of at least 1 mmol of the hydrogen or other chain transfer agent per mol of propylene for a time period, A2, wherein a concentration of the hydrogen or other chain transfer agent during time period A2 is greater than the concentration of the hydrogen or other chain transfer agent in time period A1 to form a second mode of the propylene polymer having a lower Mw with respect to the first mode; and
(e) forming a matrix of the propylene polymer, the matrix having a porosity, after time period A2, of 15% or more, as determined by mercury intrusion porosimetry.

### Claim 2 (depends on 1)

The process of claim 1, wherein the matrix after time period A2 has a median pore diameter less than 165 μm, as determined by mercury intrusion porosimetry.

### Claim 3 (depends on 1)

The process of claim 1, wherein time period A1 is at least as long as time period A2 and the concentration of the hydrogen or other chain transfer agent during time period A2 is at least three times greater than the concentration of the hydrogen or other chain transfer agent in time period A1.

### Claim 4 (depends on 1)

The process of claim 1, wherein the support has an average particle size of more than 50 μm, a surface area of less than 1000 m2/g, or a combination thereof.

### Claim 5 (depends on 1)

The process of claim 1, wherein the specific surface area is more than 650 m2/g and the mean pore diameter is less than 7 nm (70 Å).

### Claim 6 (depends on 5)

The process of claim 5, wherein the catalyst system has a bimodal particle size distribution.

### Claim 7 (depends on 6)

The process of claim 6, wherein the larger one of catalyst system modes comprises at least about 80 vol % and the smaller one of the catalyst system modes comprises at least about 5 vol %, based on the total volume of the catalyst system.

### Claim 8 (depends on 6)

The process of claim 6, wherein the propylene polymer has a bimodal particle size distribution after time period A1 or after time period A2.

### Claim 9 (depends on 1)

The process of claim 1, wherein the specific surface area is less than 650 m2/g, the mean pore diameter is greater than 7 nm (70 Å), or both.

### Claim 10 (depends on 1)

The process of claim 1, further comprising polymerizing ethylene monomer comprising ethylene and from about 3 wt % to 75 wt % of one or more C3 to C20 alpha olefins in the presence of the propylene polymer to fill pores in the matrix with a fill phase comprising from 15 to 80 wt % by total weight of the matrix and fill phase.

### Claim 11 (depends on 1)

The process of claim 1, wherein the support comprises agglomerates of primary particles.

### Claim 12 (depends on 11)

The process of claim 11, further comprising fragmenting the agglomerates in (a) and dispersing catalyst sites in the propylene polymer matrix.

### Claim 13 (depends on 1)

The process of claim 1, wherein the activator comprises alumoxane.

### Claim 14 (depends on 1)

The process of claim 1, wherein the catalyst system further comprises a co-activator selected from the group consisting of: trialkylaluminum, dialkylmagnesium, alkylmagnesium halide, and dialkylzinc.

### Claim 15 (depends on 1)

The process of claim 1, wherein the contacting of the propylene monomer with the catalyst system during time period A1, time period A2, or a combination thereof, is carried out in the liquid slurry phase.

### Claim 16 (depends on 1)

The process of claim 1, wherein the polymerization conditions during time periods Al and A2 comprise a pressure of from about 0.96 MPa (140 psi) to about 5.2 MPa (750 psi) and a temperature of from about 50° C. to 100° C.

### Claim 17 (depends on 1)

The process of claim 1, wherein the propylene monomer in (a) is essentially free of ethylene and C4 to C20 alpha olefins, and the propylene polymer formed is a propylene homopolymer.

### Claim 18 (depends on 13)

The process of claim 13, further comprising non-coordinating anion.

### Claim 19 (depends on 1)

The process of claim 1, wherein the single site catalyst precursor compound is selected from precursor compounds I and II;
wherein precursor compound I is represented by the following formula:
(Cp)mRAnM4Qk
wherein:
each Cp is a cyclopentadienyl moiety or a substituted cyclopentadienyl moiety substituted by one or more hydrocarbyl radicals having from 1 to 20 carbon atoms;
RA is a structural bridge between two Cp moieties;
M4 is a transition metal selected from groups 4 or 5;
Q is a hydride or a hydrocarbyl group having from 1 to 20 carbon atoms or an alkenyl group having from 2 to 20 carbon atoms, or a halogen;
m is 1, 2, or 3, with the proviso that if m is 2 or 3, each Cp may be the same or different;
n is 0 or 1, with the proviso that n=0 if m=1; and
k is such that k+m is equal to the oxidation state of M4, with the proviso that if k is greater than 1, each Q may be the same or different; and
wherein precursor compound II is represented by the following formula:
RA(CpR″p)(CpR*q)M5Qr
wherein:
each Cp is a cyclopentadienyl moiety or substituted cyclopentadienyl moiety;
each R* and R″ is a hydrocarbyl group having from 1 to 20 carbon atoms and may the same or different;
p is 0, 1, 2, 3, or 4;
q is 1, 2, 3, or 4;
RA is a structural bridge between the Cp moieties imparting stereorigidity to the metallocene compound;
M5 is a group 4, 5, or 6 metal;
Q is a hydrocarbyl radical having 1 to 20 carbon atoms or is a halogen;
r is s minus 2, where s is the valence of M5;
wherein (CpR*q) has bilateral or pseudobilateral symmetry; R*q is selected such that (CpR*q) forms a fluorenyl, alkyl substituted indenyl, or tetra-, tri-, or dialkyl substituted cyclopentadienyl radical; and (CpR″p) contains a bulky group in one and only one of the distal positions;
wherein the bulky group is of the formula ARwv; and
where A is chosen from group 4 metals, oxygen, or nitrogen, and Rw is a methyl radical or phenyl radical, and v is the valence of A minus 1.

### Claim 20 (depends on 1)

The process of claim 1, wherein the single site catalyst precursor compound is represented by the formula:
wherein:
M is a group 4, 5 or 6 metal;
T is a bridging group;
each X is, independently, an anionic leaving group;
each R2, R3, R4, R5, R6, R7, R8, R9, R10, R11, R12, and R13 is, independently, halogen atom, hydrogen, hydrocarbyl, substituted hydrocarbyl, halocarbyl, substituted halocarbyl, silylcarbyl, substituted silylcarbyl, germylcarbyl, substituted germylcarbyl substituent or a —NR′2, —SR′, —OR′, —OSiR′3 or —PR′2 radical, wherein R′ is one of a halogen atom, a C1-C10 alkyl group, or a C6-C10 aryl group.

### Claim 21 (depends on 20)

The process of claim 20, wherein at least one of R2, R3, R4, R5, R6, R7, R8, R9, R10, R11, R12, and R13 is a cyclopropyl substitutent represented by the formula:
wherein each R′ in the cyclopropyls substituent is, independently, hydrogen, a substituted hydrocarbyl group, an unsubstituted hydrocarbyl group, or a halogen.

### Claim 22 (depends on 20)

The process of claim 20, wherein:
M is selected from titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum and tungsten;
each X is independently selected from hydrogen, halogen, hydroxy, substituted or unsubstituted C1 to C10 alkyl groups, substituted or unsubstituted C1 to C10 alkoxy groups, substituted or unsubstituted C6 to C14 aryl groups, substituted or unsubstituted C6 to C14 aryloxy groups, substituted or unsubstituted C2 to C10 alkenyl groups, substituted or unsubstituted C7 to C40 arylalkyl groups, substituted or unsubstituted C7 to C40 alkylaryl groups and substituted or unsubstituted C7 to C40 arylalkenyl groups; or optionally are joined together to form a C4 to C40 alkanediyl group or a conjugated C4 to C40 diene ligand which is coordinated to M in a metallacyclopentene fashion; or optionally represent a conjugated diene, optionally, substituted with one or more groups independently selected from hydrocarbyl, trihydrocarbylsilyl, and trihydrocarbylsilylhydrocarbyl groups, said diene having a total of up to 40 atoms not counting hydrogen and forming a it complex with M;
each R2, R4, R8, and R10 is independently selected from hydrogen, halogen, substituted or unsubstituted C1 to C10 alkyl groups, substituted or unsubstituted C6 to C14 aryl groups, substituted or unsubstituted C2 to C10 alkenyl groups, substituted or unsubstituted C7 to C40 arylalkyl groups, substituted or unsubstituted C7 to C40 alkylaryl groups, substituted or unsubstituted C8 to C40 arylalkenyl groups, and —NR′2, —SR′, —OR′, —SiR′3, —OSiR′3, and —PR′2 radicals wherein each R′ is independently selected from halogen, substituted or unsubstituted C1 to C10 alkyl groups and substituted or unsubstituted C6 to C14 aryl groups;
R3, R5, R6, R7, R9, R11, R12, and R13 are each selected from the group consisting of hydrogen, halogen, hydroxy, substituted or unsubstituted C1 to C10 alkyl groups, substituted or unsubstituted C1 to C10 alkoxy groups, substituted or unsubstituted C6 to C14 aryl groups, substituted or unsubstituted C6 to C14 aryloxy groups, substituted or unsubstituted C2 to C10 alkenyl groups, substituted or unsubstituted C7 to C40 arylalkyl groups, substituted or unsubstituted C7 to C40 alkylaryl groups and C7 to C40 substituted or unsubstituted arylalkenyl groups; and
T is selected from:
—B(R14)—, —Al(R14)—, —Ge—, —Sn—, —O—, —S—, —SO—, —SO2—, —N(R14)—, —CO—, —P(R14)—, and —P(O)(R14)—;
wherein R14, R15, and R16 are each independently selected from hydrogen, halogen, C1 to C20 alkyl groups, C6 to C30 aryl groups, C1 to C20 alkoxy groups, C2 to C20 alkenyl groups, C7 to C40 arylalkyl groups, C8 to C40 arylalkenyl groups and C7 to C40 alkylaryl groups, optionally R14 and R15, together with the atom(s) connecting them, form a ring; and M3 is selected from carbon, silicon, germanium, and tin; or
T is represented by the formula:
wherein R17, R18, R19, R20, R21, R22, R23, and R24 are each independently selected from hydrogen, halogen, hydroxy, substituted or unsubstituted C1 to C10 alkyl groups, substituted or unsubstituted C1 to C10 alkoxy groups, substituted or unsubstituted C6 to C14 aryl groups, substituted or unsubstituted C6 to C14 aryloxy groups, substituted or unsubstituted C2 to C10 alkenyl groups, substituted or unsubstituted C7 to C40 alkylaryl groups, substituted or unsubstituted C7 to C40 alkylaryl groups and substituted or unsubstituted C8 to C40 arylalkenyl groups; optionally two or more adjacent radicals R17, R18, R19, R20, R21, R22, R23, and R24, including R20 and R21, together with the atoms connecting them, form one or more rings; and
M2 represents one or more carbon atoms, or a silicon, germanium, or tin atom.

### Claim 23

A propylene polymer comprising:
at least 50 mol % propylene;
a 1% Secant flexural modulus of at least 1000 MPa, determined according to ASTM D 790 (A, 1.0 mm/min);
more than 5 and less than 200 regio defects per 10,000 propylene units, determined by 13C NMR;
a multimodal molecular weight distribution;
if comonomer is present, a CDBI of 50% or more; and
a matrix having a porosity of 15 percent or more, and median pore diameter less than 165 μm, as determined by mercury intrusion porosimetry.

### Claim 24 (depends on 23)

The propylene polymer of claim 23, wherein the median pore diameter is from 0.1 up to 160 μm.

### Claim 25 (depends on 23)

The propylene polymer of claim 23, further comprising:
a total propylene content of at least 75 wt %;
if comonomer is present, a total co-monomer content from about 3 wt % up to about 25 wt %;
if comonomer is present, a CDBI of at least 60%;
a matrix porosity of at least 35%;
a matrix median pore diameter greater than 8 μm and less than 150 μm, as determined by mercury intrusion porosimetry;
at least 50% isotactic pentads;
more than 10 regio defects per 10,000 propylene units, determined by 13C NMR;
a 1% Secant flexural modulus of at least 1800 MPa;
a melting point (Tm, DSC peak second melt) of at least 145° C.;
an Mw/Mn as measured by GPC-DRI of greater than 1 up to 5;
an overall Mw/Mn of greater than 1 to 20 and at least one mode having an Mw/Mn of greater than 1 to 5;
at least 95% by volume having a particle size greater than 150 μm up to 10 mm;
a melt flow rate (MFR, ASTM 1238, 230° C., 2.16 kg) from about 0.1 dg/min up to about 300 dg/min;
an Mw (as measured by GPC-DRI) from 50,000 to 1,000,000 g/mol; or
a combination thereof.