# US 2016/0354870 A1 · Welded joint and method of manufacturing welded joint

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0354870 A1
- Document ID: US20160354870A1
- Status: Published application
- Kind: A1
- Application number: 15/117,467
- Filed: 2015-02-20
- Published: 2016-12-08
- Earliest claimed: 2014-02-26
- Assignees: Nippon Steel & Sumitomo Metal Corporation
- Applicants: Nippon Steel & Sumitomo Metal Corporation
- Inventors: Kana JOTOKU; Hiroyuki HIRATA; Tomohiko OMURA; Jun NAKAMURA; Takihiro OSUKI
- Web page: https://patentgrep.com/patent/US20160354870A1

## CPC

- B23K 35/3066: {with Ni as next major constituent}
- B23K 9/167: and of a non-consumable electrode
- B23K 9/173: and of a consumable electrode
- B23K 9/23: taking account of the properties of the materials to be welded
- B23K 35/0227: {Rods or wires (B23K35/0244 takes precedence)}
- B23K 35/3086: {containing Ni or Mn}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/58: with more than 1.5% by weight of manganese
- F16L 9/02: of metal (F16L9/16 - F16L9/22 take precedence)
- B23K 2101/10: Pipe-lines
- B23K 2103/04: Steel {or steel} alloys
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F16L: PIPES; JOINTS OR FITTINGS FOR PIPES; SUPPORTS FOR PIPES, CABLES OR PROTECTIVE TUBING; MEANS FOR THERMAL INSULATION IN GENERAL

## Abstract

A welded joint having high strength and good hydrogen embrittlement resistance is provided. A welded joint is a welded joint obtained by welding a base material using a welding material. The base material has a chemical composition of, in mass %: C: 0.005 to 0.1%; Si: up to 1.2%; Mn: 2.5 to 6.5%; Ni: 8 to 15%; Cr: 19 to 25%; Mo: 0.01 to 4.5%; V: 0.01 to 0.5%; Nb: 0.01 to 0.5% Al: less than 0.05%; N: 0.15 to 0.45%; O: up to 0.02%; P: up to 0.05%; and S: up to 0.04%, and a balance being iron and impurities, and which satisfies Equation (1). The welding material has a chemical composition which satisfies Equations (1) and (2). Ni+0.65Cr+0.98Mo+1.05Mn+0.35Si+12.6C≧29 (1) 0.31C+0.048Si—0.02Mn−0.056Cr+0.007Ni−0.013Mo≦−1.0 (2)

## Claims

### Claim 1

A welded joint obtained by welding a base material using a welding material, wherein the base material has a chemical composition of, in mass %:
C: 0.005 to 0.1%;
Si: up to 1.2%;
Mn: 2.5 to 6.5%;
Ni: 8 to 15%;
Cr: 19 to 25%;
Mo: 0.01 to 4.5%;
V: 0.01 to 0.5%;
Nb: 0.01 to 0.5%;
Al: less than 0.05%;
N: 0.15 to 0.45%;
O: up to 0.02%;
P: up to 0.05%; and
S: up to 0.04%, and
a balance being iron and impurities,
wherein the welding material has a chemical composition of, in mass %:
C: 0.005 to 0.1%;
Si: up to 0.7%;
Mn: 0.5 to 3%;
Ni: 8 to 23%;
Cr: 17 to 25%;
Mo: 0.01 to 4%;
V: 0 to 0.5%;
Nb: 0 to 0.5%;
Al: less than 0.05%;
N: less than 0.15%;
O: up to 0.02%;
P: up to 0.03%; and
S: up to 0.02%, and
a balance being iron and impurities,
wherein the chemical composition of the base material satisfies Equation (1), and
the chemical composition of the welding material satisfies Equations (1) and (2),
Ni+0.65Cr+0.98Mo+1.05Mn+0.35Si+12.6C≧29 (1), and
0.31C+0.048Si−0.02Mn−0.056Cr+0.007Ni−0.013Mo≦−1.0 (2),
where the contents of elements (in mass %) are substituted for the symbols of these elements in Equations (1) and (2).

### Claim 2 (depends on 1)

The welded joint according to claim 1, wherein the chemical composition of the welding material includes one or more selected from the group consisting of, in mass %:
V: 0.01 to 0.5%; and
Nb: 0.01 to 0.5%.

### Claim 3 (depends on 1)

The welded joint according to claim 1, having a surface excess weld metal height h (mm) that satisfies Equation (3),
1.9×(0.31C+0.048Si−0.02Mn−0.056Cr+0.007Ni−0.013Mo)+3≦h (3),
where the contents of the elements in the welding material (in mass %) are substituted for the symbols of these elements in Equation (3).

### Claim 4 (depends on 1)

The welded joint according to claim 1, having a tensile strength of 800 MPa or higher.

### Claim 5

A method of manufacturing a welded joint, comprising the steps of:
preparing a base material having a chemical composition of, in mass %:
C: 0.005 to 0.1%;
Si: up to 1.2%;
Mn: 2.5 to 6.5%;
Ni: 8 to 15%;
Cr: 19 to 25%;
Mo: 0.01 to 4.5%;
V: 0.01 to 0.5%;
Nb: 0.01 to 0.5%;
Al: less than 0.05%;
N: 0.15 to 0.45%;
O: up to 0.02%;
P: up to 0.05%; and
S: up to 0.04%, and
a balance being iron and impurities,
preparing a welding material having a chemical composition of, in mass %:
C: 0.005 to 0.1%;
Si: up to 0.7%;
Mn: 0.5 to 3%;
Ni: 8 to 23%;
Cr: 17 to 25%;
Mo: 0.01 to 4%;
V: 0 to 0.5%;
Nb: 0 to 0.5%;
Al: less than 0.05%;
N: less than 0.15%;
O: up to 0.02%;
P: up to 0.03%; and
S: up to 0.02%, and
a balance being iron and impurities, and
welding the base material using the welding material,
wherein the chemical composition of the base material satisfies Equation (1), and
the chemical composition of the welding material satisfies Equations (1) and (2),
Ni+0.65Cr+0.98Mo+1.05Mn+0.35Si−12.6C≧29 (1), and
0.31C+0.048Si−0.02Mn−0.056Cr+0.007Ni−0.013Mo≦−1.0 (2),
where the contents of elements (in mass %) are substituted for the symbols of these elements in Equations (1) and (2).

### Claim 6 (depends on 2)

The welded joint according to claim 2, having a surface excess weld metal height h (mm) that satisfies Equation (3),
1.9×(0.31C+0.048Si−0.02Mn−0.056Cr+0.007Ni−0.013Mo)+3≦h (3),
where the contents of the elements in the welding material (in mass %) are substituted for the symbols of these elements in Equation (3).

### Claim 7 (depends on 2)

The welded joint according to claim 2, having a tensile strength of 800 MPa or higher.

### Claim 8 (depends on 3)

The welded joint according to claim 3, having a tensile strength of 800 MPa or higher.

### Claim 9 (depends on 6)

The welded joint according to claim 6, having a tensile strength of 800 MPa or higher.