# US 2016/0251744 A1 · Bearing steel

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0251744 A1
- Document ID: US20160251744A1
- Status: Published application
- Kind: A1
- Application number: 15/052,883
- Filed: 2016-02-25
- Published: 2016-09-01
- Earliest claimed: 2015-02-27
- Assignees: Aktiebolaget Skf
- Inventors: Hanzheng HUANG; Mohamed SHERIF
- Web page: https://patentgrep.com/patent/US20160251744A1

## CPC

- C22C 38/58: with more than 1.5% by weight of manganese
- C21D 1/20: Isothermal quenching, e.g. bainitic hardening
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/007: {containing Co}
- C21D 6/008: {containing Si}
- C21D 9/36: for balls; for rollers
- C21D 9/40: for rings; for bearing races
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/52: with cobalt
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 1/613: Gases; Liquefied or solidified normally gaseous material
- C21D 6/02: Hardening by precipitation
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/004: Dispersions; Precipitations
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A steel alloy for a bearing, the alloy having a composition comprising: (a) from 0.5 to 0.9 wt. % carbon, (b) from 1.2 to 1.8 wt. % silicon, (c) from 1.1 to 1.7 wt. % manganese, (d) from 0.7 to 1.3 wt. % chromium, (e) from 0.05 to 0.6 wt. % molybdenum, and optionally any of: (fl) from 0 to 0.25 wt. % nickel, (f2) from 0 to 0.02 wt. % vanadium, (f3) from 0 to 0.05 wt. % aluminium, (f4) from 0 to 0.3 wt. % copper, (f5) from 0 to 0.5 wt. % cobalt, (f6) from 0 to 0.1 wt. % niobium, (f7) from 0 to 0.1 wt. % tantalum, (f7) from 0 to 150 ppm nitrogen, (f8) from 0 to 50 ppm calcium, and (f9) the balance iron, together with any unavoidable impurities, wherein the steel alloy has a microstructure comprising bainitic ferrite and retained austenite, and a hardness (Vickers) of at least 650 HV.

## Claims

### Claim 1

A method of heat-treating a steel alloy comprising steps of:
(i) providing a steel alloy composition comprising:
from 0.5 to 0.9 wt. % carbon,
from 1.2 to 1.8 wt. % silicon,
from 1.1 to 1.7 wt. % manganese,
from 0.7 to 1.3 wt. % chromium,
from 0.05 to 0.6 wt. % molybdenum,
from 0 to 0.25 wt. % nickel,
from 0 to 0.02 wt. % vanadium,
from 0 to 0.05 wt. % aluminium,
from 0 to 0.3 wt. % copper,
from 0 to 0.5 wt. % cobalt,
from 0 to 0.1 wt. % niobium,
from 0 to 0.1 wt. % tantalum,
from 0 to 150 ppm nitrogen,
from 0 to 50 ppm calcium,
the balance iron, together with any unavoidable impurities,
(ii) heating the composition to a temperature of at least 865° C. to at least partially austenitise the composition;
(iii) quenching the composition to a first temperature T1, wherein 0.7Ms≦T1≦1.6Ms, Ms being the martensite start temperature of the austenite composition; and
(iv) heating the composition to a second temperature T2 below the bainite start temperature of the austenite composition Bs.

### Claim 2 (depends on 1)

The method of claim 1, wherein T1 is above the martensite start temperature.

### Claim 3 (depends on 1)

The method of claim 1, wherein T1 is from 190 to 210° C.

### Claim 4 (depends on 1)

The method of claim 1, wherein, during step (iii), the composition is held at T1 for at least 5 hours.

### Claim 5 (depends on 1)

The method of claim 1, wherein T1 is below the martensite start temperature Ms.

### Claim 6 (depends on 1)

The method of claim 1, wherein T2 is from 50 to 150° C. below the bainite start temperature.

### Claim 7 (depends on 1)

The method of claim 1, wherein T2 is from 220 to 280° C.

### Claim 8 (depends on 1)

The method of claim 1, wherein step (ii) is carried out at a temperature of from 865 to 950° C.

### Claim 9 (depends on 1)

The method of claim 1, wherein step (ii) is carried out at for a time of at least 30 minutes.

### Claim 10 (depends on 1)

The method of claim 1, wherein, during step (iv), the composition is heated isothermally.

### Claim 11 (depends on 1)

The method of claim 1, further comprising a step of:
(v) cooling the composition to room temperature.

### Claim 12 (depends on 1)

The method of claim 1, further comprising a step of:
(vi) cooling the composition to a temperature of less than 0° C.

### Claim 13 (depends on 1)

The method of claim 1, further comprising a step of:
(vii) tempering at a temperature of from 100 to 200° C. for at least one hour.

### Claim 14 (depends on 1)

The method of claim 1, further comprising a step of:
(viii) subjecting the steel alloy to a surface finishing technique.

### Claim 15 (depends on 1)

The method of claim 1, further comprising forming the steel alloy into a bearing component.

### Claim 16 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.6 to 0.8 wt. % carbon.

### Claim 17 (depends on 1)

The method of claim 1, wherein the alloy comprises from 1.3 to 1.7 wt. % silicon.

### Claim 18 (depends on 1)

The method of claim 1, wherein the alloy comprises from 1.2 to 1.6 wt. % manganese.

### Claim 19 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.8 to 1.2 wt. % chromium.

### Claim 20 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.07 to 0.4 wt. % molybdenum.

### Claim 21 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.003 to 0.02 wt. % vanadium.

### Claim 22 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.05 to 0.25 wt. % nickel.

### Claim 23 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.05 to 0.3 wt. % copper.

### Claim 24 (depends on 1)

The method of claim 1, wherein the alloy comprises from 0.005 to 0.05 wt. % aluminium.

### Claim 25 (depends on 1)

The method of claim 1, wherein the alloy comprises from 50 to 150 ppm nitrogen.

### Claim 26 (depends on 1)

The method of claim 1, wherein the heat-treated alloy has a microstructure comprising nano-structured bainitic ferrite and retained austenite.

### Claim 27 (depends on 26)

The method of claim 26, wherein the alloy comprises at least 80 vol. % bainite.

### Claim 28 (depends on 26)

The method of claim 26, wherein the alloy comprises less than 15 vol. % retained austenite.

### Claim 29 (depends on 26)

The method of claim 26, wherein the alloy comprises wherein the microstructure comprises plates of bainitic-ferrite of less than 200 nm.

### Claim 30 (depends on 26)

The method of claim 26, wherein the alloy comprises having a hardness (Vickers) of at least 650 HV.