# US 2016/0250779 A1 · Peroxide cross-linking and high temperature melting

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0250779 A1
- Document ID: US20160250779A1
- Status: Published application
- Kind: A1
- Application number: 15/030,206
- Filed: 2014-10-16
- Published: 2016-09-01
- Earliest claimed: 2013-10-17
- Assignees: The General Hospital Corporation
- Applicants: The General Hospital Corporation
- Inventors: Orhun K. Muratoglu; Ebru Oral
- Web page: https://patentgrep.com/patent/US20160250779A1

## CPC

- B29C 35/0805: {using electromagnetic radiation}
- A61F 2/0095: {Packages or dispensers for prostheses or other implants (for intraocular lenses A61F2/1691; for dental surgery A61C19/02)}
- B29B 7/88: Adding charges {, i.e. additives}
- B29B 11/06: by moulding the material
- B29B 11/12: Compression moulding
- B29B 13/022: {Melting the material to be shaped}
- B29B 13/045: {of powders or pellets}
- B29C 35/02: Heating or curing, e.g. crosslinking or vulcanizing {during moulding, e.g. in a mould}(cold vulcanisation B29C35/18 {; vulcanising tyres, presses therefor B29D30/0601})
- B29C 35/0866: {using particle radiation}
- B29C 43/006: {Pressing and sintering powders, granules or fibres}
- B29C 43/10: Isostatic pressing, i.e. using non-rigid pressure-exerting members against rigid parts or dies
- B65B 31/00: Packaging articles or materials under special atmospheric or gaseous conditions; Adding propellants to aerosol containers
- B65B 55/08: by irradiation
- B65B 55/10: by liquids or gases
- B65B 55/16: by irradiation
- B65B 55/18: by liquids or gases (B65B55/14 takes precedence)
- C08J 3/203: {Solid polymers with solid and/or liquid additives}
- C08J 3/24: Crosslinking, e.g. vulcanising, of macromolecules (mechanical aspects B29C35/00; crosslinking agents C08K)
- C08J 7/12: Chemical modification
- C08J 7/123: {Treatment by wave energy or particle radiation (C08J7/18 takes precedence)}
- B29B 2013/002: {Extracting undesirable residual components, e.g. solvents, unreacted monomers, from material to be moulded}
- B29C 2035/085: {using gamma-ray}
- B29C 2035/0877: {using electron radiation, e.g. beta-rays}
- B29C 2071/022: {Annealing}
- B29C 2791/001: Shaping in several steps
- B29C 2791/002: Making articles of definite length, i.e. discrete articles (B29C53/40 takes precedence)
- B29K 2023/0683: {UHMWPE, i.e. ultra high molecular weight polyethylene}
- B29K 2105/0035: {Medical or pharmaceutical agents}
- B29K 2995/0087: Wear resistance
- B29L 2009/00: Layered products
- B29L 2031/7532: {Artificial members, protheses}
- C08J 2323/06: Polyethene
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- A61F: FILTERS IMPLANTABLE INTO BLOOD VESSELS; PROSTHESES; DEVICES PROVIDING PATENCY TO, OR PREVENTING COLLAPSING OF, TUBULAR STRUCTURES OF THE BODY, e.g. STENTS; ORTHOPAEDIC, NURSING OR CONTRACEPTIVE DEVICES; FOMENTATION; TREATMENT OR PROTECTION OF EYES OR EARS; BANDAGES, DRESSINGS OR ABSORBENT PADS; FIRST-AID KITS (dental prosthetics A61C)
- B29B: PREPARATION OR PRETREATMENT OF THE MATERIAL TO BE SHAPED; MAKING GRANULES OR PREFORMS; RECOVERY OF PLASTICS OR OTHER CONSTITUENTS OF WASTE MATERIAL CONTAINING PLASTICS
- B65B: MACHINES, APPARATUS OR DEVICES FOR, OR METHODS OF, PACKAGING ARTICLES OR MATERIALS; UNPACKING (bundling and pressing devices for cigars A24C1/44; devices for tensioning and securing binders adapted to be supported by the article or articles to be bound B25B25/00; applying closure members to bottles, jars or similar containers B67B1/00-B67B6/00; concurrent cleaning, filling and closing of bottles B67C7/00; emptying bottles, jars, cans, casks, barrels or similar containers B67C9/00)
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29L: INDEXING SCHEME ASSOCIATED WITH SUBCLASS B29C, RELATING TO PARTICULAR ARTICLES

## Abstract

Methods of making oxidation and wear resistant polymeric materials using peroxide cross-linking and high temperature melting process are disclosed. A multiple step procedure for enabling the manufacturing of such material without size limitations is also disclosed.

## Claims

### Claim 1

A method of making a consolidated polymeric material comprising:
blending the polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material; and
completely consolidating the pre-molded, heat treated blended polymeric material.

### Claim 2

A method of making a consolidated polymeric material comprising:
blending the polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form under hydrostatic pressure below 200° C., followed by completely consolidating by heating the pre-molded polymeric material to a temperature above 200° C. for a period of time under hydrostatic pressure; and
cooling the completely consolidated premolded blended polymeric material.

### Claim 3

A method of making a consolidated polymeric material comprising:
blending the polymeric material with one or more additives;
consolidating the polymeric material blend under hydrostatic pressure above 200° C.; and
cooling the completely consolidated blended polymeric material.

### Claim 4

A method of making a cross-linked consolidated polymeric material comprising: blending the polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material;
completely consolidating the pre-molded, heat treated blended polymeric material; and
irradiating the consolidated polymeric material.

### Claim 5

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded blended polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material;
completely consolidating the pre-molded, heat treated blended polymeric material;
machining the consolidated polymeric material into implant shape; and
irradiating the medical implant.

### Claim 6

A method of making a cross-linked consolidated polymeric material comprising blending the polymeric material with one or more additives, pre-molding the blended polymeric material into a partially consolidated form, heating the pre-molded polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time, cooling the pre-molded blended polymeric material, completely consolidating the pre-molded, heat treated blended polymeric material, irradiating the consolidated polymeric material and heating the irradiated consolidated polymeric material.

### Claim 7

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded blended polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material;
completely consolidating the pre-molded, heat treated blended polymeric material;
machining the consolidated polymeric material into a medical implant shape: and
irradiating the medical implant.

### Claim 8

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded blended polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material;
completely consolidating the pre-molded, heat treated blended polymeric material;
irradiating the consolidated polymeric material;
heating the irradiated consolidated polymeric material; and
cooling, machining the irradiated consolidated material into implant shape.

### Claim 9

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded blended polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material; and
completely consolidating the pre-molded, heat treated blended polymeric material into implant shape by direct compression molding.

### Claim 10

A method of making a interlocked hybrid medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded blended polymeric material to a temperature above the melting temperature of the blended polymeric material for a period of time;
cooling the pre-molded blended polymeric material; and
completely consolidating the pre-molded, heat treated blended polymeric material into implant shape by direct compression molding onto a second material.

### Claim 11

A method of making a cross-linked consolidated polymeric material comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded polymeric material to a temperature above the melting temperature of the polymeric material for a period of time;
cooling the pre-molded polymeric material;
completely consolidating the pre-molded, heat treated polymeric material;
irradiating the consolidated polymeric material;
machining the irradiated consolidated polymeric material;
diffusing the implant preform with one or more additives; and
heating and subsequently cooling the diffused implant preform.

### Claim 12

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into a partially consolidated form;
heating the pre-molded polymeric material to a temperature above the melting temperature of the polymeric material for a period of time;
cooling the pre-molded polymeric material;
completely consolidating the pre-molded, heat treated polymeric material;
irradiating the consolidated polymeric material;
machining the irradiated consolidated polymeric material into a medical implant perform;
diffusing the implant preform with one or more additives; and
heating the diffused implant preform and subsequently cooling and machining into implant shape.

### Claim 13

A method of making a consolidated polymeric material comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into partially consolidated form;
heating the pre-molded polymeric material to a temperature above its melting temperature of the polymeric material for a period of time;
cooling the pre-molded polymeric material;
layering the pre-molded polymeric material with a layer of a cross-link agent-blended pre-molded or resin polymeric material; and
completely consolidating the layered material.

### Claim 14

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into partially consolidated form;
heating the pre-molded polymeric material to a temperature above its melting temperature of the polymeric material for a period of time;
cooling the pre-molded polymeric material;
layering the pre-molded polymeric material with more than one layer of cross-link agent-blended pre-molded or resin polymeric material; and
completely consolidating the layered material.

### Claim 15

A method of making a medical implant comprising:
blending a polymeric material with one or more additives;
pre-molding the blended polymeric material into partially consolidated form;
heating the pre-molded polymeric material to a temperature above its melting temperature of the polymeric material for a period of time;
cooling the pre-molded polymeric material;
layering the pre-molded polymeric material with a layer of a cross-link agent-blended pre-molded or resin polymeric material; and
completely consolidating the layered material.

### Claim 16 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12)

The method according to any of claims 1-12, wherein the additive is an antioxidant.

### Claim 17 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16)

The method according to any of claims 1-16, wherein the additive is a cross-linking agent.

### Claim 18 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16)

The method according to any of claims 1-16, wherein the additive is vitamin E.

### Claim 19 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16)

The method according to any of claims 1-16, wherein the additive is a peroxide.

### Claim 20 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-19 or 21-61, wherein the polymeric material is irradiated after the complete consolidation step.

### Claim 21 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 22, 45, 46, 47, 48, 49, 50, 60, 61)

The method according to any of claim 4-8, 11, 12, 20, 22, 45-50 or 60-61, wherein the irradiated polymeric material is further heated below the melting point of the irradiated polymeric material.

### Claim 22 (depends on 4, 5, 6, 7, 8, 11, 12, 20)

The method according to any of claim 4-8, 11, 12, 20, or 21, 45-50 or 60-61, wherein the irradiated polymeric material is further heated above the melting point of the irradiated polymeric material.

### Claim 23 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-22 or 24-61, wherein the polymeric material is heated below or above the melting point of the polymeric material.

### Claim 24 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-23 or 25-61, wherein the complete consolidation step is carried out by compression molding, direct compression molding, uniaxial compression, or hot isostatic pressing.

### Claim 25 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-24 or 16-61, wherein the polymeric material is blended with one or more antioxidants.

### Claim 26 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-25 or 27-61, wherein the polymeric material is blended with vitamin E.

### Claim 27 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-26 or 28-61, wherein the polymeric material is chosen from high-density-polyethylene, low-density-polyethylene, linear-low-density-polyethylene, ultra-high molecular weight polyethylene (UHMWPE), copolymers or mixtures thereof.

### Claim 28 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15 or 29-40, wherein the pre-molding is done by compression.

### Claim 29 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28 or 30-40, wherein the pre-molding is done by isostatic pressure or hydrostatic pressure.

### Claim 30 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28, 29 or 31-40, wherein the pre-molding is done at a temperature between room temperature and the peak melting temperature of the polymeric material.

### Claim 31

The method according to any of claim, 1, 2, 4-15, 28-30 or 32-40, wherein the pre-molding is done at a temperature close to the peak melting temperature of the polymeric material.

### Claim 32 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 31, 33, 34, 35, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28, 29, 31 or 33-40, wherein the pre-molding is done at a temperature above the peak melting temperature of the polymeric material.

### Claim 33 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 30, 31, 32, 34, 35, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28-32 or 34-40, wherein the pre-molding is done at below the ambient pressure.

### Claim 34 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 30, 31, 32, 33, 35, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28-33 or 35-40, wherein the pre-molding is done under vacuum.

### Claim 35 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 30, 31, 32, 33, 34, 36, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28-34 or 36-40, wherein the pre-molding is done under about 1, 2, 3, 4, 5 MPa or more of uniaxial or hydrostatic pressure.

### Claim 36 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 30, 31, 32, 33, 34, 35, 37, 38, 39, 40)

The method according to any of claim 1, 2, 4-15, 28-35 or 37-40, wherein the heat treatment after pre-molding is done at a temperature above 200° C.

### Claim 37 (depends on 36)

The method according to claim 36, wherein the heat treatment after pre-molding is done at a temperature between 280 and 330° C.

### Claim 38 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 39, 40)

The method according to any of claim 1, 2, 4-15, 28-37 or 39-40, wherein the heat treatment after pre-molding is done for at least 1 hour up to 1 week.

### Claim 39 (depends on 38)

The method according to claim 38, wherein the heat treatment after pre-molding is done for between 2 and 8 hours.

### Claim 40 (depends on 1, 2, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39)

The method according to any of claim 1, 2, 4-15 or 28-39, wherein the heat treatment after pre-molding is done in inert gas, or a mixture of inert gas and air.

### Claim 41 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-40 or 42-61, wherein the complete consolidation step is done by compression.

### Claim 42 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-41 or 43-61, wherein the complete consolidation step is done by applying isostatic or hydrostatic pressure.

### Claim 43 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-42 or 44-61, wherein the complete consolidation is done above the peak melting temperature of the polymeric material and a pressure from 0.1 to 1000 MPa.

### Claim 44 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61)

The method according to any of claim 1-43 or 45-61, wherein the complete consolidation is done at a temperature between 170 and 230° C. and a pressure between 10 and 25 MPa.

### Claim 45 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 46, 47, 48, 49, 50, 58, 59, 60, 61)

The method according to any of claim 4-8, 11, 12, 20-22 or 46-50 or 58-61, wherein the irradiation is an electron beam irradiation.

### Claim 46 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 47, 48, 49, 50, 58, 59, 60, 61)

The method according to any of claim 4-8, 11, 12 or 20-22, 45, 47-50 or 58-61, wherein the irradiation is a gamma irradiation.

### Claim 47 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 48, 49, 50, 58, 59, 60, 61)

The method according to any of claim 4-8, 11, 12, 20-22, 45, 46, 48-50 or 58-61, wherein the irradiation is performed at about room temperature.

### Claim 48 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 47, 49, 50, 58, 59, 60, 61)

The method according to any of claim 4-8, 11, 12, 20-22, 45-47, 49, 50 or 58-61, wherein the irradiation is performed at an elevated temperature below the melting point of the polymeric material.

### Claim 49 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 47, 48, 50, 58, 59, 60, 61)

The method according to any of claim 4-8, 11, 12, 20-22, 45-48, 50 or 58-61, wherein the irradiation is performed at an elevated temperature close to the peak melting temperature of the polymeric material.

### Claim 50 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 47, 48, 49)

The method according to any of claim 4-8, 11, 12, 20-22, 45-49, or 58-61, wherein the irradiation is performed at an elevated temperature above the melting temperature of the polymeric material.

### Claim 51 (depends on 10)

The method according to claim 10, wherein the second material in the complete consolidation to form a interlocked hybrid material is a porous metal.

### Claim 52 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62)

The method according to any of claim 1-51 or 53-62, wherein the final polymeric material is machined into an implant.

### Claim 53 (depends on 52)

The method according to claim 52, wherein the medical implant is packaged and sterilized.

### Claim 54 (depends on 53)

The method according to claim 53, wherein the packaging is done in inert gas or partial inert gas.

### Claim 55 (depends on 53)

The method according to claim 53, wherein the packaging is done in vacuum.

### Claim 56 (depends on 53)

The method according to claim 53, wherein the sterilization is a gamma sterilization.

### Claim 57 (depends on 53)

The method according to claim 53, wherein the sterilization is a gas sterilization.

### Claim 58 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 47, 48, 49, 50, 60, 61)

A method according to any of claim 4-8, 11, 12, 20-22, 45-50 or 60-61, wherein the heating after irradiation is done below the peak melting temperature of the polymeric material.

### Claim 59 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 47, 48, 49, 50, 60, 61)

A method according to any of claim 4-8, 11, 12, 20-22, 45-50 or 60-61, wherein the heating after irradiation is done above the peak melting temperature of the polymeric material.

### Claim 60 (depends on 4, 5, 6, 7, 8, 11, 12, 20, 21, 22, 45, 46, 47, 48, 49, 50, 58, 59)

The method according to any of claim 4-8, 11, 12, 20-22, 45-50, 58 or 59, wherein the irradiation is to a dose of 0.1 kGy to 1000 kGy.

### Claim 61 (depends on 60)

The method according to claim 60, wherein the irradiation is to a dose of 150 or 175 kGy.

### Claim 62

The method according to any of claims wherein the cooling step is optional.

### Claim 63 (depends on 13, 14, 15)

The method according to any of claims 13-15, wherein the consolidated layered material is machined into final implant shape.

### Claim 64 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63)

The method according to any of claims 1-63, wherein the complete consolidation step is done by direct compression molding.

### Claim 65 (depends on 64)

Method according to claim 64 wherein the direct compression molded layered material chain is formed into final implant shape.

### Claim 66

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent;
b. consolidating the blended polymeric material;
c. heating the consolidated polymeric material to a temperature below or above its melting temperature and maintaining for a period of time;
d. heating the consolidated polymeric material to another temperature below or above its melting temperature and maintaining for a period of time; and
e. cooling the heated consolidated polymeric material.

### Claim 67

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent;
b. heating the consolidated polymeric material to a temperature below or above its melting temperature and maintaining for a period of time;
c. heating the consolidated polymeric material to another temperature below or above its melting temperature and maintaining for a period of time;
d. cooling the heated consolidated polymeric material to a temperature above the melting temperature and maintaining for a period of time;
e. cooling the heated consolidated polymeric material to another temperature below the melting temperature and maintaining for a period of time; and
f. further cooling the heated consolidated polymeric material.

### Claim 68

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a carbon-carbon initiator; and
b. consolidating the blended polymeric material.

### Claim 69 (depends on 66, 67, 68)

The method of claim 66, 67 or 68, wherein the consolidation is done between 180 and 210° C.

### Claim 70 (depends on 66, 67, 68)

The method of claim 66, 67 or 68, wherein the consolidation is done between 180 and 350° C.

### Claim 71 (depends on 66, 67, 68)

The method of claim 66, 67 or 68, wherein at least one antioxidant is vitamin E.

### Claim 72 (depends on 66, 67, 68)

The method of claim 66, 67 or 68, wherein at least one cross-linking agent is a peroxide.

### Claim 73 (depends on 66)

The method according to claim 66, wherein the consolidated polymeric material is heated to below the peak melting temperature of the consolidated polymeric material.

### Claim 74 (depends on 66)

The method according to claim 66, wherein steps c and d can be performed multiple times in any sequence.

### Claim 75 (depends on 66, 67, 68)

The method according to claim 66, 67 or 68, wherein the cross-linked polymeric material is further machined into a medical implant.

### Claim 76 (depends on 66, 67, 68)

A medical implant made by the methods according to any of the claim 66, 67 or 68.

### Claim 77 (depends on 76)

The method according to claim 76, wherein the medical implant is packaged and sterilized.

### Claim 78 (depends on 66, 67, 68)

The method according to claim 66, 67 or 68, wherein the consolidation is done by ram extrusion.

### Claim 79

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent;
b. consolidating the blended polymeric material;
c. heating the consolidated polymeric material to a temperature to between about 200° C. and about 290° C.;
d. maintaining the consolidated polymeric material between about 200° C. and about 290° C. for at least 4 hours;
e. heating the consolidated polymeric material to a temperature between about 290° C. and 350° C.;
f. maintaining the consolidated polymeric material between about 290° C. and 350° C. for at least 5 hours but no more than 30 hours;
g. cooling the heated consolidated polymeric material to a temperature between about 135° C. and about 180° C.;
h. maintaining the consolidated polymeric material between about 135° C. and about 180° C.; and
i. cooling the consolidated polymeric material to between about room temperature and 60° C.

### Claim 80 (depends on 79)

The method according to claim 79, wherein at least one antioxidant is vitamin E.

### Claim 81 (depends on 79)

The method according to claim 79, wherein at least one cross-linking agent is a peroxide.

### Claim 82 (depends on 79)

The method according to claim 79, wherein at least one cross-linking agent is P130.

### Claim 83 (depends on 66, 67, 68, 79)

The method according to claim 66, 67, 68 or 79, wherein at least one cross-linking agent is Trigonox 311.

### Claim 84 (depends on 66, 67)

The method according to claims 66, 67, or 79, wherein at least one cross-linking agent is a carbon-carbon initiator.

### Claim 85 (depends on 66, 67, 68, 79)

The method according to claim 66, 67, 68 or 79, wherein the heating after consolidation is done in inert gas.

### Claim 86 (depends on 66, 67, 68, 79)

The method according to claim 66, 67, 68 or 79, wherein the heating after consolidation is done in air.

### Claim 87

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent;
b. consolidating the blended polymeric material;
c. heating the consolidated polymeric material;
d. extracting byproducts from the consolidated polymeric material; and
e. cooling the extracted consolidated polymeric material.

### Claim 88

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent;
b. consolidating the blended polymeric material;
c. heating the consolidated polymeric material;
d. cooling the consolidated polymeric material; and
e. extracting byproducts from the consolidated polymeric material.

### Claim 89 (depends on 87, 88)

The method according to claim 87 or 88, wherein the extraction is done in water.

### Claim 90 (depends on 87, 88)

The method according to claims 87 and 88, wherein the extraction is done in inert gas.

### Claim 91 (depends on 87, 88)

The method according to claims 87 and 88, wherein the extraction is done in air.

### Claim 92 (depends on 87, 88)

The method according to claims 87 and 88, wherein at least one antioxidant is vitamin E.

### Claim 93 (depends on 87, 88)

The method according to claims 87 and 88, wherein at least one cross-linking agent is a peroxide.

### Claim 94 (depends on 87, 88)

The method according to claims 87 and 88, wherein at least one cross-linking agent is P130.

### Claim 95 (depends on 87, 88)

The method according to claims 87 and 88, wherein machining into a medical implant is performed before or after extraction.

### Claim 96 (depends on 95)

The method according to claim 95, wherein the medical implant is packaged and sterilized.

### Claim 97

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. partially consolidating the blended polymeric material;
c. high temperature melting the partially consolidated, blended polymeric material;
d. consolidating the high temperature melted, partially consolidated, blended polymeric material; and
e. irradiating the consolidated, blended polymeric material.

### Claim 98

A method of making a cross-linked polymeric material, the method comprising:
a. blending a polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. consolidating the blended polymeric material;
c. high temperature melting the consolidated, blended polymeric material;
d. consolidating the high temperature melted, partially consolidated, blended polymeric material; and
e. irradiating the consolidated, blended polymeric material.

### Claim 99 (depends on 97, 98)

The method according to claims 97 and 98, wherein the cross-linked polymeric material is heated to temperature(s) between room temperature and the peak melting temperature of the cross-linked polymeric material and maintained for a period of time before cooling down to about room temperature.

### Claim 100 (depends on 97, 98)

The method according to claim 97 or 98, wherein the cross-linked polymeric material is heated to temperature(s) above the peak melting temperature of the cross-linked polymeric material and maintained for a period of time before cooling down to about room temperature.

### Claim 101 (depends on 97, 98)

The method according to claim 97 or 98, wherein the cross-linked polymeric material is machined into a medical implant.

### Claim 102 (depends on 97)

The method according to claim 97, wherein the consolidated polymeric material is machined into a medical implant before irradiation.

### Claim 103 (depends on 101, 102)

The method according to claim 101 or 102, wherein the medical implant is packaged and sterilized.

### Claim 104 (depends on 97, 98)

The method according to claim 97 or 98, wherein at least one additive is vitamin E.

### Claim 105 (depends on 97, 98)

The method according to claim 97 or 98, wherein at least one consolidation is done by compression molding.

### Claim 106 (depends on 97, 98)

The method according to claim 97 or 98, wherein at least one consolidation is done by isostatic pressing.

### Claim 107 (depends on 97, 98)

The method according to claim 97 or 98, wherein at least one consolidation is done by ram extrusion or ram compression.

### Claim 108

A method of making a cross-linked polymeric material, the method comprising;
a. blending a first polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. partially consolidating the first blended polymeric material;
c. high temperature melting the partially consolidated, blended polymeric material;
d. blending a second polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent; and
e. layering the partially consolidated, blended polymeric material and the second blended polymeric material and consolidating the layers, thereby forming a layered cross-linked polymeric material.

### Claim 109 (depends on 108)

The method according to claim 108, wherein the layered cross-linked polymeric material is heated to temperature(s) between room temperature and the peak melting temperature of the polymeric material.

### Claim 110 (depends on 108)

The method according to claim 108, wherein the layered cross-linked polymeric material is heated to temperature(s) above the peak melting temperature of the polymeric material.

### Claim 111

A method of making a cross-linked polymeric material, the method comprising:
a. blending a first polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. partially consolidating the first blended polymeric material;
c. blending a second polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent; and
d. layering the partially consolidated, blended polymeric material and the second blended polymeric material and consolidating the layers, thereby forming a layered cross-linked polymeric material.

### Claim 112

A method of making a cross-linked polymeric material, the method comprising:
a. blending a first polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. bending a second polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent; and
c. layering the first blended polymeric material and the second blended polymeric material and consolidating the layers, thereby forming a layered cross-linked polymeric material.

### Claim 113

A method of making a cross-linked polymeric material, the method comprising:
a. blending a first polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. partially consolidating the first blended polymeric material;
c. blending a second polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent;
d. Partially consolidating the second blended polymeric material; and
e. layering the first and second partially consolidated, blended polymeric materials and consolidating the layers, thereby forming a layered cross-linked polymeric material.

### Claim 114 (depends on 108, 111, 112, 113)

The method according to claim 108, 111, 112 or 113, wherein more blends of polymeric material with one more additive(s) are layered before consolidation.

### Claim 115

A method of making an interlocked hybrid material, the method comprising:
a. blending a first polymeric material with one or more additive(s) at least one of which is an antioxidant;
b. partially consolidating the first blended polymeric material;
c. blending a second polymeric material with one or more additive(s) at least one of which is an antioxidant and at least one of which is a cross-linking agent; and
d. layering the partially consolidated, blended polymeric material and the second blended polymeric material and a third material consolidating the layers, thereby forming an interlocked, hybrid material.

### Claim 116 (depends on 115)

The method according to claim 115, wherein the third material is a metal.

### Claim 117 (depends on 115)

The method according to claim 115, wherein the third material is a porous metal.

### Claim 118 (depends on 108, 111, 112, 113, 115)

The method according to claim 108, 111, 112, 113 or 115, wherein the cross-linked polymeric material or interlocked hybrid material is consolidated in the form of a medical implant.

### Claim 119 (depends on 108, 111, 112, 113, 115)

The method according to claim 108, 111, 112, 113 or 115, wherein the cross-linked polymeric material or the interlocked hybrid material is machined into a medical implant.

### Claim 120 (depends on 118, 119)

The method according to claim 118 or 119, wherein the medical implant is packaged and sterilized.

### Claim 121 (depends on 108, 111, 112, 113, 115)

The method according to claim 108, 111, 112, 113 or 115, wherein at least one additive in the polymeric blends is an antioxidant.

### Claim 122 (depends on 108, 111, 112, 113, 115)

The method according to claim 108, 111, 112, 113 or 115, wherein at least one additive in the polymeric blends is vitamin E.

### Claim 123 (depends on 108, 111, 112, 113, 115)

The method according to claim 108, 111, 112, 113 or 115, wherein at least one cross-linking agent in the polymeric blends is P130.

### Claim 124 (depends on 66, 67, 68, 79, 87, 88, 97, 98, 108, 111, 112, 113, 115)

The method according to any of claim 66, 67, 68, 79, 87, 88, 97, 98, 108, 111, 112, 113 or 115, wherein the antioxidant concentration is between 0.05 wt % and 66.0 wt %.

### Claim 125 (depends on 66, 67, 79, 87, 88, 108, 111, 112, 113, 115)

The method according to any of claim 66, 67, 79, 87, 88, 108, 111, 112, 113 or 115, wherein the cross-linking agent or cross-linking initiator concentration is between 0.5 and 66.5 wt %.

### Claim 126 (depends on 98)

The method according to claim 98, wherein the antioxidant concentration is 0.2 wt % and the irradiation dose is 150 kGy.

### Claim 127 (depends on 98)

The method according to claim 98, wherein the irradiated polymeric material is heated to below the melting temperature.

### Claim 128 (depends on 98)

The method according to claim 98, wherein the irradiated polymeric material is heated to above the melting temperature.

### Claim 129 (depends on 77, 98, 103, 120)

The method according to any of claim 77, 98, 103 or 120, wherein sterilization is done by irradiation and/or by gas sterilization.

### Claim 130 (depends on 77, 98, 103, 120)

The method according to any of claim 77, 98, 103 or 120, wherein the medical implant is cleaned before packaging and sterilization.

### Claim 131 (depends on 97, 98)

The method according to claim 97 or 98, wherein irradiation is a gamma irradiation or an electron beam irradiation.

### Claim 132 (depends on 66, 67, 79, 87, 88, 108, 111, 112, 113, 115)

A medical implant made by a method according to any of claim 66, 67, 79, 87, 88, 108, 111, 112, 113 or 115.