# US 2016/0250683 A1 · Secondary cast aluminum alloy for structural applications

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0250683 A1
- Document ID: US20160250683A1
- Status: Published application
- Kind: A1
- Application number: 14/632,308
- Filed: 2015-02-26
- Published: 2016-09-01
- Earliest claimed: 2015-02-26
- Assignees: GM Global Technology Operations LLC
- Applicants: GM Global Technology Operations LLC
- Inventors: Qigui Wang; Jason R. Traub; Michael J. Walker; Anil K. Sachdev
- Web page: https://patentgrep.com/patent/US20160250683A1

## CPC

- B22D 21/007: {with low melting point, e.g. Al 659 degrees C, Mg 650 degrees C}
- B22D 25/02: by its peculiarity of shape; of works of art {(cylinders, pistons B22D15/02)}
- C22C 21/02: with silicon as the next major constituent
- C22C 21/12: with copper as the next major constituent
- C22C 21/16: with magnesium
- C22C 21/18: with zinc
- C22F 1/043: of alloys with silicon as the next major constituent
- C22F 1/057: of alloys with copper as the next major constituent
- G01N 33/20: Metals
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- G01N: INVESTIGATING OR ANALYSING MATERIALS BY DETERMINING THEIR CHEMICAL OR PHYSICAL PROPERTIES (measuring or testing apparatus or processes other than immunoassay, involving enzymes or microorganisms C12M, C12Q)

## Abstract

An aluminum alloy that can be cast into structural components wherein at least some of the raw materials used to produce the alloy are sourced from secondary production sources. In addition to aluminum as the primary constituent, such an alloy includes 5 to 14% silicon, 0 to 1.5% copper, 0.2 to 0.55% magnesium, 0.2 to 1.2% iron, 0.1 to 0.6% manganese, 0 to 0.5% nickel, 0 to 0.8% zinc, 0 to 0.2% of other trace elements selected from the group consisting essentially of titanium, zirconium, vanadium, molybdenum and cobalt. In a preferred form, most of the aluminum is from a secondary production source. Methods of analyzing a secondary production aluminum alloy to determine its constituent makeup is also disclosed, as is a method of adjusting the constituent makeup of such an alloy in situations where the alloy is out of tolerance when measured against its primary source counterpart.

## Claims

### Claim 1

An aluminum alloy consisting essentially of raw materials by weight approximately 5 to 14% silicon, 0 to 1.5% copper, 0.2 to 0.55% magnesium, 0.2 to 1.2% iron, 0.1 to 0.6% manganese, 0 to 0.5% nickel, 0 to 0.8% zinc, 0 to 0.2% of other trace elements selected from the group consisting essentially of titanium, zirconium, vanadium, molybdenum and cobalt, and the balance aluminum, wherein at least a portion of said balance aluminum comprises secondary production aluminum.

### Claim 2 (depends on 1)

The aluminum alloy of claim 1, wherein at least a majority of said balance aluminum comprises secondary production aluminum.

### Claim 3 (depends on 1)

The aluminum alloy of claim 1, wherein a substantial entirety of said balance aluminum comprises secondary production aluminum.

### Claim 4 (depends on 1)

The aluminum alloy of claim 1, wherein said silicon is by weight approximately 5 to 8%, said copper is by weight approximately 0 to 1.0%, said magnesium is by weight approximately 0.2 to 0.4%, said iron is by weight no more than approximately 0.4%, said manganese is by weight approximately 0 to 0.2%, said nickel is by weight approximately 0 to 0.2% and said zinc is by weight approximately 0 to 0.3%.

### Claim 5 (depends on 1)

The aluminum alloy of claim 1, wherein said silicon is by weight approximately 8 to 14%, said copper is by weight approximately 1.0 to 1.5%, said magnesium is by weight approximately 0.4 to 0.55%, said iron is by weight no more than approximately 0.8%, said manganese is by weight approximately 0 to 0.3%, said nickel is by weight approximately 0 to 0.5% and said zinc is by weight approximately 0 to 0.5%.

### Claim 6 (depends on 1)

The aluminum alloy of claim 1, wherein said copper and said magnesium by weight are below approximately 0.5% and 0.2%, respectively.

### Claim 7

A method of forming a cast automotive component, said method comprising:
heating a quantity of raw materials at least a portion of which comprises secondary production raw materials until at least a substantial majority thereof melts to become by weight approximately 5 to 14% silicon, 0 to 1.5% copper, 0.2 to 0.55% magnesium, 0.2 to 1.2% iron, 0.1 to 0.6% manganese, 0 to 0.5% nickel, 0 to 0.8% zinc, 0 to 0.2% of other trace elements selected from the group consisting essentially of titanium, zirconium, vanadium, molybdenum and cobalt, and the balance aluminum;
placing said heated quantity of raw material into a mold that substantially defines the shape of said component; and
cooling said melted quantity of raw materials.

### Claim 8 (depends on 7)

The method of claim 7, further comprising:
determining whether the presence of at least one alloying ingredient is within tolerance;
and adjusting an amount of at least one of said alloying ingredients that is outside said tolerance.

### Claim 9 (depends on 7)

The method of claim 7, wherein said component is selected from the group consisting of an engine block and cylinder head.

### Claim 10 (depends on 9)

The method of claim 9, wherein said aluminum alloy comprises at least one of a high ductility alloy or a high fatigue strength alloy wherein said silicon is by weight approximately 5 to 8%, said copper is by weight approximately 0 to 1.0%, said magnesium is by weight approximately 0.2 to 0.4%, said iron is by weight no more than approximately 0.4%, said manganese is by weight approximately 0 to 0.2%, said nickel is by weight approximately 0 to 0.2% and said zinc is by weight approximately 0 to 0.3%.

### Claim 11 (depends on 9)

The method of claim 9, wherein said aluminum alloy comprises a high tensile strength alloy wherein said silicon is by weight approximately 8 to 14%, said copper is by weight approximately 1.0 to 1.5%, said magnesium is by weight approximately 0.4 to 0.55%, said iron is by weight no more than approximately 0.8%, said manganese is by weight approximately 0 to 0.3%, said nickel is by weight approximately 0 to 0.5% and said zinc is by weight approximately 0 to 0.5%.

### Claim 12 (depends on 9)

The method of claim 9, wherein said aluminum alloy comprises a high pressure die cast alloy wherein said copper and said magnesium by weight are below approximately 0.5% and 0.2%, respectively.

### Claim 13 (depends on 7)

The method of claim 7, wherein at least a majority of said balance aluminum comprises secondary production aluminum.

### Claim 14 (depends on 7)

The method of claim 7, wherein said mold is selected from the group consisting of a sand mold, lost foam mold, die cast mold, permanent (gravity) mold or combinations thereof.

### Claim 15 (depends on 7)

The method of claim 7, wherein said heating takes place in a furnace and said cooling takes place in a mold.

### Claim 16 (depends on 7)

The method of claim 7, wherein said heating comprises overheating in order to substantially eliminate any residual atomic cluster that may be present in said heated quantity of raw material.

### Claim 17

A method of verifying the casting quality of an aluminum alloy, the method comprising:
receiving a sample of said aluminum alloy at least a portion of which comprises secondary production raw materials;
generating a microstructure image corresponding to a location of interest in said sample;
measuring at least one indicia within said image; and
correlating said indicia with the presence of at least alloy constituent or at least one contaminant within said alloy.

### Claim 18 (depends on 17)

The method of claim 17, wherein at least one of said receiving, generating and measuring comprises performing a metallographic analysis.

### Claim 19 (depends on 18)

The method of claim 18, wherein said metallographic analysis is performed by a microstructure image analysis system with at least one algorithm programmed therein to measure at least one phase fraction.

### Claim 20 (depends on 17)

The method of claim 17, wherein said at least a portion of said secondary production raw materials comprises a majority by weight of secondary production aluminum.

### Claim 21 (depends on 17)

The method of claim 17, wherein said aluminum alloy consists essentially of by weight approximately 5 to 14% silicon, 0 to 1.5% copper, 0.2 to 0.55% magnesium, 0.2 to 1.2% iron, 0.1 to 0.6% manganese, 0 to 0.5% nickel, 0 to 0.8% zinc, 0 to 0.2% of other trace elements selected from the group consisting essentially of titanium, zirconium, vanadium, molybdenum and cobalt, and the balance aluminum.

### Claim 22 (depends on 17)

The method of claim 17, wherein said indicia comprises an iron intermetallic phase volume fraction.