# US 2016/0240313 A1 · COG Dielectric Composition For Use With Nickel Electrodes

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0240313 A1
- Document ID: US20160240313A1
- Status: Published application
- Kind: A1
- Application number: 15/024,166
- Filed: 2014-09-08
- Published: 2016-08-18
- Earliest claimed: 2013-10-30
- Assignees: Ferro Corporation
- Applicants: Ferro Corporation
- Inventors: Walter J. Symes, Jr.
- Web page: https://patentgrep.com/patent/US20160240313A1

## CPC

- H01G 4/1245: {containing also titanates}
- B32B 18/00: Layered products essentially comprising ceramics, e.g. refractory products
- C04B 35/486: Fine ceramics
- C04B 35/49: containing also titanium oxides or titanates
- C04B 35/491: based on lead zirconates and lead titanates {, e.g. PZT}
- C04B 35/6261: {Milling}
- H01G 4/0085: {Fried electrodes}
- H01G 4/01: Form of self-supporting electrodes
- H01G 4/12: Ceramic dielectrics {(H01G4/085 takes precedence)}
- H01G 4/1236: {based on zirconium oxides or zirconates (H01G4/1263 takes precedence)}
- H01G 4/30: Stacked capacitors (H01G4/33 takes precedence)
- C04B 2235/3206: Magnesium oxides or oxide-forming salts thereof
- C04B 2235/3208: Calcium oxide or oxide-forming salts thereof, e.g. lime
- C04B 2235/3213: Strontium oxides or oxide-forming salts thereof
- C04B 2235/3224: Rare earth oxide or oxide forming salts thereof, e.g. scandium oxide
- C04B 2235/3232: Titanium oxides or titanates, e.g. rutile or anatase
- C04B 2235/3236: Alkaline earth titanates
- C04B 2235/3244: Zirconium oxides, zirconates, hafnium oxides, hafnates, or oxide-forming salts thereof
- C04B 2235/3248: Zirconates or hafnates, e.g. zircon
- C04B 2235/3251: Niobium oxides, niobates, tantalum oxides, tantalates, or oxide-forming salts thereof
- C04B 2235/3255: Niobates or tantalates, e.g. silver niobate
- C04B 2235/3262: Manganese oxides, manganates, rhenium oxides or oxide-forming salts thereof, e.g. MnO
- C04B 2235/3409: Boron oxide, borates, boric acids, or oxide forming salts thereof, e.g. borax
- C04B 2235/5445: submicron sized, i.e. from 0,1 to 1 micron
- C04B 2235/6025: Tape casting, e.g. with a doctor blade
- C04B 2235/6582: Hydrogen containing atmosphere
- C04B 2235/6584: at an oxygen percentage below that of air
- C04B 2235/6588: Water vapor containing atmospheres
- C04B 2237/348: Zirconia, hafnia, zirconates or hafnates
- C04B 2237/68: Forming laminates or joining articles wherein at least one substrate contains at least two different parts of macro-size, e.g. one ceramic substrate layer containing an embedded conductor or electrode
- H01G: CAPACITORS; CAPACITORS, RECTIFIERS, DETECTORS, SWITCHING DEVICES, LIGHT-SENSITIVE OR TEMPERATURE-SENSITIVE DEVICES OF THE ELECTROLYTIC TYPE (selection of specified materials as dielectric H01B3/00; capacitors having potential barriers H10D1/62, H10K10/10)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE

## Abstract

Multilayer ceramic chip capacitors which satisfy COG requirements and which are compatible with reducing atmosphere sintering conditions so that non-noble metals such as nickel and nickel alloys may be used for internal and external electrodes are disclosed. The capacitors exhibit desirable dielectric properties (high capacitance, low dissipation factor, high insulation resistance), excellent performance on highly accelerated life testing, and very good resistance to dielectric breakdown. The dielectric layers comprise a strontium zirconate matrix doped with other metal oxides such as TiO2, MgO, B2O3, CaO, MnO, Nd2O3 and Nb2O5 in various combinations.

## Claims

### Claim at position 1

1: A composition comprising a mixture of precursor materials that, upon firing, forms a dielectric material comprising a strontium-zirconate matrix doped with at least niobium, boron and magnesium.

### Claim at position 2 (depends on 1)

2: The composition according to claim 1, wherein the dielectric material exhibits a dielectric constant greater than 31.

### Claim at position 3 (depends on 1)

3: The composition according to claim 1, wherein the mixture further comprises precursor materials such that, upon firing, result in the dielectric material further comprising one or more dopants selected from the group consisting of titanium, calcium, neodymium, and manganese.

### Claim at position 4

4: A lead-free and cadmium-free dielectric material comprising a solids portion wherein the solids portion comprises, prior to firing:
from about 38.3 wt % to about 44.2 wt % SrO;
from about 41.6 wt % to about 50.0 wt % ZrO2;
optionally up to about 4.8 wt % TiO2;
optionally up to about 3.2 wt % CaO;
from about 6.4 wt % to about 7.6 wt % Nb2O5;
optionally up to about 4.1 wt % Nd2O3;
from about 0.27 wt % to about 0.38 wt % B2O3;
from about 0.31 wt % to about 0.44 wt % MgO; and
optionally up to about 0.06 wt % MnO.

### Claim at position 5 (depends on 4)

5: A method of forming an electronic component comprising:
applying the dielectric material of claim 4 to a substrate; and
firing the substrate at a temperature sufficient to sinter the dielectric material.

### Claim at position 6 (depends on 5)

6: The method of claim 5, wherein the firing is conducted at a temperature of from about 1200° C. to about 1350° C.

### Claim at position 7 (depends on 5)

7: The method of claim 5, wherein the firing is conducted in an atmosphere having a partial oxygen pressure of about 10−12 atm to about 10−8 atm.

### Claim at position 8 (depends on 4)

8: A multilayer ceramic chip capacitor comprising a fired collection of:
alternately stacked layers of:
the dielectric material of claim 4; and
layers of an internal electrode material comprising a transition metal other than Ag, Au, Pd, or Pt.

### Claim at position 9 (depends on 8)

9: The multilayer ceramic chip capacitor of claim 8, wherein the internal electrode material comprises nickel.

### Claim at position 10 (depends on 4)

10: A method of forming an electronic component comprising:
alternately applying layers of
the dielectric material of claim 4, and
a metal-containing electrode paste
onto a substrate to form a laminar stack;
firing the substrate at a temperature sufficient to sinter the dielectric material;
cutting the laminar stack to a predetermined shape;
separating the cut stack from the substrate; and
firing the stack to sinter the metal in the electrode paste and fuse the oxides in the dielectric material, wherein the electrode layers and the dielectric material layers each have layer thicknesses.

### Claim at position 11 (depends on 10)

11: The method of claim 10, wherein the layers of dielectric material, after firing, each have a thickness of about 1 microns to about 50 microns.

### Claim at position 12 (depends on 10)

12: The method of claim 10, wherein the firing is conducted at a temperature of from about 1200° C. to about 1325° C.

### Claim at position 13 (depends on 10)

13: The method of claim 10, wherein the firing is conducted in an atmosphere having a partial oxygen pressure of about 10−12 atm to about 10−8 atm.

### Claim at position 14 (depends on 10)

14: The method of claim 10, wherein the metal-containing electrode paste comprises nickel.

### Claim at position 15

16: A lead-free and cadmium-free dielectric material comprising a solids portion wherein the solids portion comprises, prior to firing:
from about 54.6 wt % to about 63.0 wt % SrCO3;
from about 41.6 wt % to about 50.0 wt % ZrO2;
optionally up to about 4.8 wt % TiO2;
optionally up to about 5.7 wt % CaCO3;
from about 6.4 wt % to about 7.6 wt % Nb2O5;
optionally up to about 4.1 wt % Nd2O3;
from about 0.27 wt % to about 0.38 wt % B2O3;
from about 0.31 wt % to about 0.44 wt % MgO; and
optionally up to about 0.06 wt % MnO.

### Claim at position 16 (depends on 15)

16: A method of forming an electronic component comprising:
applying the dielectric material of claim 15 to a substrate; and
firing the substrate at a temperature sufficient to sinter the dielectric material.

### Claim at position 17 (depends on 16)

17: The method of claim 16, wherein the firing is conducted at a temperature of from about 1200° C. to about 1350° C.

### Claim at position 18 (depends on 16)

18: The method of claim 16, wherein the firing is conducted in an atmosphere having a partial oxygen pressure of about 10−12 atm to about 10−8 atm.

### Claim at position 19 (depends on 15)

19: A multilayer ceramic chip capacitor comprising a fired collection of:
alternately stacked layers of:
the dielectric material of claim 15; and
layers of an internal electrode material comprising a transition metal other than Ag, Au, Pd, or Pt.

### Claim at position 20 (depends on 19)

20: The multilayer ceramic chip capacitor of claim 19, wherein the internal electrode material comprises nickel.

### Claim at position 21 (depends on 15)

21: A method of forming an electronic component comprising:
alternately applying layers of
the dielectric material comprising of claim 15, and
a metal-containing electrode paste
onto a substrate to form a laminar stack;
firing the substrate at a temperature sufficient to sinter the dielectric material;
cutting the laminar stack to a predetermined shape;
separating the cut stack from the substrate; and
firing the stack to sinter the metal in the electrode paste and fuse the oxides in the dielectric material, wherein the electrode layers and the dielectric material layers each have layer thicknesses.

### Claim at position 22 (depends on 21)

22: The method of claim 21, wherein the layers of dielectric material, after firing, each have a thickness of about 1 microns to about 50 microns.

### Claim at position 23 (depends on 21)

23: The method of claim 21, wherein the firing is conducted at a temperature of from about 1200° C. to about 1325° C.

### Claim at position 24 (depends on 21)

24: The method of claim 21, wherein the firing is conducted in an atmosphere having a partial oxygen pressure of about 10−12 atm to about 10−8 atm.

### Claim at position 25 (depends on 21)

25: The method of claim 21, wherein the metal-containing electrode paste comprises nickel.

### Claim at position 26

26: A lead-free and cadmium-free dielectric material comprising a solids portion wherein the solids portion comprises, prior to firing:
optionally up to about 1.3 SrTiO3;
from about 70.8 wt % to about 81.7 wt % SrZrO3;
optionally up to about 3.4 wt % CaZrO3;
optionally up to about 7.6 wt % CaTiO3;
from about 11.6 wt % to about 13.5 wt % Sr2Nb2O7;
optionally up to about 7.1 wt % Nd2ZrO5;
from about 0.27 wt % to about 0.38 wt % B2O3;
from about 0.31 wt % to about 0.44 wt % MgO; and
optionally up to about 0.06 wt % MnO.

### Claim at position 27 (depends on 26)

27: A method of forming an electronic component comprising:
applying the dielectric material of claim 26 to a substrate; and
firing the substrate at a temperature sufficient to sinter the dielectric material.

### Claim at position 28 (depends on 27)

28: The method of claim 27, wherein the firing is conducted at a temperature of from about 1200° C. to about 1350° C.

### Claim at position 29 (depends on 27)

29: The method of claim 27, wherein the firing is conducted in an atmosphere having a partial oxygen pressure of about 10−12 atm to about 10−8 atm.

### Claim at position 30 (depends on 26)

30: A multilayer ceramic chip capacitor comprising a fired collection of:
alternately stacked layers of:
the dielectric material of claim 26; and
layers of an internal electrode material comprising a transition metal other than Ag, Au, Pd, or Pt.

### Claim at position 31 (depends on 30)

31: The multilayer ceramic chip capacitor of claim 30, wherein the internal electrode material comprises nickel.

### Claim at position 32 (depends on 26)

32: A method of forming an electronic component comprising:
alternately applying layers of
the dielectric material of claim 26, and
a metal-containing electrode paste
onto a substrate to form a laminar stack;
firing the substrate at a temperature sufficient to sinter the dielectric material;
cutting the laminar stack to a predetermined shape;
separating the cut stack from the substrate; and
firing the stack to sinter the metal in the electrode paste and fuse the oxides in the dielectric material, wherein the electrode layers and the dielectric material layers each have layer thicknesses.

### Claim at position 33 (depends on 32)

33: The method of claim 32, wherein the layers of dielectric material, after firing, each have a thickness of about 1 microns to about 50 microns.

### Claim at position 34 (depends on 32)

34: The method of claim 32, wherein the firing is conducted at a temperature of from about 1200° C. to about 1325° C.

### Claim at position 35 (depends on 32)

35: The method of claim 32, wherein the firing is conducted in an atmosphere having a partial oxygen pressure of about 10−12 atm to about 10−8 atm.

### Claim at position 36 (depends on 32)

36: The method of claim 32, wherein the metal-containing electrode paste comprises nickel.