# US 2016/0236965 A1 · Ultralow expansion titania-silica glass

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0236965 A1
- Document ID: US20160236965A1
- Status: Published application
- Kind: A1
- Application number: 15/003,115
- Filed: 2016-01-21
- Published: 2016-08-18
- Earliest claimed: 2015-02-13
- Assignees: Corning Incorporated
- Applicants: Corning Incorporated
- Inventors: Sezhian Annamalai; Carlos Alberto Duran; Kenneth Edward Hrdina; William Rogers Rosch
- Web page: https://patentgrep.com/patent/US20160236965A1

## CPC

- C03C 3/076: with 40% to 90% silica, by weight {(C03C3/045 takes precedence)}
- C03B 19/12: by liquid-phase reaction processes
- C03B 19/1453: {Thermal after-treatment of the shaped article, e.g. dehydrating, consolidating, sintering}
- C03B 25/00: Annealing glass products
- C03B 25/02: in a discontinuous way
- C03C 3/06: with more than 90% silica by weight, e.g. quartz {(C03C3/045 takes precedence)}
- C03C 3/089: containing boron
- C03C 3/112: containing fluorine
- C03C 23/007: {by thermal treatment}
- C03B 2201/10: doped with boron (C03B2201/14 takes precedence)
- C03B 2201/12: doped with fluorine (C03B2201/14 takes precedence)
- C03B 2201/42: doped with titanium
- C03C 2201/10: containing boron (C03C2201/14 takes precedence)
- C03C 2201/12: containing fluorine (C03C2201/14 takes precedence)
- C03C 2201/14: containing boron and fluorine
- C03C 2203/52: Heat-treatment
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C03B: MANUFACTURE, SHAPING, OR SUPPLEMENTARY PROCESSES

## Abstract

Annealing treatments for modified titania-silica glasses and the glasses produced by the annealing treatments. The annealing treatments include an isothermal hold that facilitates equalization of non-uniformities in fictive temperature caused by non-uniformities in modifier concentration in the glasses. The annealing treatments may also include heating the glass to a higher temperature following the isothermal hold and holding the glass at that temperature for several hours. Glasses produced by the annealing treatments exhibit high spatial uniformity of CTE, CTE slope, and fictive temperature, including in the presence of a spatially non-uniform concentration of modifier.

## Claims

### Claim 1

A method of annealing glass comprising:
heating a modified titania-silica glass to a first temperature, said modified titania-silica glass including a non-uniform concentration of a modifier, said first temperature exceeding 850° C.;
cooling said modified titania-silica glass at a first cooling rate from said first temperature to a second temperature, said second temperature being in the range from 650° C. to 800° C.; and
holding said modified titania-silica glass at said second temperature for a first time period, said first time period lasting for at least 10 hours.

### Claim 2 (depends on 1)

The method of claim 1, wherein said modifier is F or B2O3.

### Claim 3 (depends on 1)

The method of claim 1, wherein said non-uniform modifier concentration includes a peak-to-valley variation of at least 0.10 wt %.

### Claim 4 (depends on 1)

The method of claim 1, wherein said first cooling rate is 1° C./hr or greater.

### Claim 5 (depends on 1)

The method of claim 1, further comprising cooling said modified titania-silica glass at a second cooling rate from said second temperature to a third temperature, said second cooling rate exceeding 50° C./hr and said third temperature being at least 300° C. less than said second temperature.

### Claim 6 (depends on 1)

The method of claim 1, further comprising heating said modified titania-silica glass from said second temperature to a third temperature, said third temperature exceeding said second temperature by no more than 25° C.

### Claim 7 (depends on 6)

The method of claim 6, further comprising holding said modified titania-silica glass at said third temperature for a second period of time, said second period of time lasting at least 5 hours.

### Claim 8

A method of annealing glass comprising:
heating a modified titania-silica glass to a first temperature, said modified titania-silica glass including a non-uniform concentration of a modifier, said first temperature exceeding 850° C.;
cooling said modified titania-silica glass at a first cooling rate from said first temperature to a second temperature, said second temperature being in the range from 650° C. to 800° C.;
cooling said modified titania-silica glass at a second cooling rate from said second temperature to a third temperature, said second cooling rate being less than 1° C./hr, said cooling at said second cooling rate occurring for at least 10 hours.

### Claim 9 (depends on 8)

The method of claim 8, wherein said third temperature is no more than 10° C. less than said second temperature.

### Claim 10 (depends on 9)

The method of claim 9, further comprising heating said modified titania-silica glass from said third temperature to a fourth temperature, said fourth temperature being in the range from 5° C. to 25° C. greater than said third temperature.

### Claim 11

An article comprising a glass, said glass having a composition comprising:
7.0 wt %-13.0 wt % TiO2;
79.0 wt %-92.9 wt % SiO2; and
0.1 wt %-8.0 wt % modifier;
wherein said glass has an average CTE slope at 20° C. of less than 1.2 ppb/K2; and
wherein said glass has a non-uniform coefficient of thermal expansion at 20° C., said non-uniform coefficient of thermal expansion including a maximum coefficient of thermal expansion and a minimum coefficient of thermal expansion, the difference between said maximum coefficient of thermal expansion and said minimum coefficient of thermal expansion not exceeding 5 ppb/K; and
wherein said glass has a non-uniform modifier concentration, said non-uniform modifier concentration including a maximum modifier concentration and a minimum modifier concentration, the difference between said maximum modifier concentration and said minimum modifier concentration exceeding 0.03 wt %.

### Claim 12 (depends on 11)

The article of claim 11, wherein said modifier is F or B2O3.

### Claim 13 (depends on 11)

The article of claim 11, wherein said modifier is B2O3 and said glass comprises 2.0 wt %-6.0 wt % of said modifier.

### Claim 14 (depends on 11)

The article of claim 11, wherein said difference between said maximum coefficient of thermal expansion and said minimum coefficient of thermal expansion does not exceed 2 ppb/K.

### Claim 15 (depends on 14)

The article of claim 14, wherein said difference between said maximum modifier concentration and said minimum modifier concentration exceeds 0.05 wt %.

### Claim 16 (depends on 15)

The article of claim 15, wherein said difference between said maximum coefficient of thermal expansion and said minimum coefficient of thermal expansion does not exceed 1 ppb/K.

### Claim 17 (depends on 16)

The article of claim 16, wherein said glass comprises 0.5 wt %-7.5 wt % of said modifier and said difference between said maximum modifier concentration and said minimum modifier concentration exceeds 0.10 wt %.

### Claim 18 (depends on 11)

The article of claim 11, wherein said difference between said maximum coefficient of thermal expansion and said minimum coefficient of thermal expansion does not exceed 3 ppb/K and said difference between said maximum modifier concentration and said minimum modifier concentration exceeds 0.05 wt %.

### Claim 19

An article comprising a glass, said glass having a composition comprising:
7.0 wt %-13.0 wt % TiO2;
at least 79.0 wt % SiO2; and
a modifier, said modifier having an average concentration of at least 0.1 wt %, said glass having an average CTE slope at 20° C. less than 1.2 ppb/K2; said glass including a first region and a second region, said first region having a first fictive temperature and a concentration of said modifier at least 0.03 wt % greater than said average modifier concentration, said second region having a second fictive temperature and a concentration of said modifier at least 0.03 wt % less than said average modifier concentration, said first fictive temperature exceeding said second fictive temperature.

### Claim 20 (depends on 19)

The article of claim 19, wherein said average concentration of said modifier is at least 0.5 wt %.

### Claim 21 (depends on 19)

The article of claim 19, wherein said first region has a concentration of said modifier at least 0.05 wt % greater than said average modifier concentration and said second region has a concentration of said modifier at least 0.05 wt % less than said average modifier concentration

### Claim 22 (depends on 19)

The article of claim 19, wherein said average modifier concentration is at least 0.2 wt % and said first region has a concentration of said modifier at least 0.10 wt % greater than said average modifier concentration and said second region has a concentration of said modifier at least 0.10 wt % less than said average modifier concentration.

### Claim 23 (depends on 19)

The article of claim 19, wherein said first fictive temperature exceeds said second fictive temperature by at least 1° C.